Hand Files Cut With a Double-Edged Hammer and Tempered in Burnt Ox Horn and Salt (Theophilus, 12th Century)
Forge

Tạo bởi

Forge

14. tháng Mười Một 2026NO
13
0
0
0
0

Hand Files Cut With a Double-Edged Hammer and Tempered in Burnt Ox Horn and Salt (Theophilus, 12th Century)

How a medieval metalworker made his own files, from Theophilus's De Diversis Artibus (12th century): files of steel, or of soft iron faced with steel, forged to size, smoothed and cut with a double-edged hammer or cutting iron, then hardened by sprinkling them glowing with burnt ox horn and salt and quenching. Small soft-iron files are packed in lard, goatskin and clay instead.
Nâng cao
About 1 day per few files

Hướng dẫn

1

The hardening mix

Đang tải sổ tay Jupyter…
2

Read De Diversis Artibus, Book III

"Files are made from pure steel, large and moderately sized, triangular and round. Others also are made which are stronger in the middle, from soft iron inside, but outwardly they are covered with steel."
3

Forge and smooth the blanks

Beat steel (or soft iron covered with steel) to the size and shape wanted: large or moderate, triangular or round; for small files, square, round, triangular or thin. Smooth them on a planing instrument (a filing or scraping bed).

Vật liệu cho bước này:

Thanh thép cacbon (0,6 % C)Thanh thép cacbon (0,6 % C)1 cái
Thanh sắt rènThanh sắt rèn1 cái

Công cụ cần thiết:

Lò rènLò rèn
Bễ thổiBễ thổi
ĐeĐe
BúaBúa
Kìm rènKìm rèn
Giũa (giũa tay)Giũa (giũa tay)
4

Cut the teeth

Mark out the teeth with a hammer sharp on both sides, or with the cutting iron, until the file is cut all over.

Công cụ cần thiết:

BúaBúa
Đục khắc giũaĐục khắc giũa
ĐeĐe
Ê tô bàn nguộiÊ tô bàn nguội
5

Temper with horn and salt

Burn an ox horn in the fire, scrape it, mix it with a third part of salt and grind it hard. Heat the file until it glows, sprinkle the mixture over it everywhere, lay hot coals on and blow quickly over the whole without letting the coating fall off; then draw it out and quench it evenly in water, and dry it slightly over the fire. He tempers all steel things this way.

Vật liệu cho bước này:

Sừng bòSừng bò1 cái
MuốiMuối1 cái

Công cụ cần thiết:

Lò rènLò rèn
Bễ thổiBễ thổi
PipetPipet
Kìm rènKìm rèn
Thùng tôi nướcThùng tôi nước
6

Or pack small soft-iron files

For small soft-iron files, after cutting, anoint them with the grease of an old hog, bind them with small straps of buck-goat skin tied with flaxen thread, and cover each with beaten clay, leaving the handles (tangs) bare. Dry them, put them in the fire and blow strongly until the skin is burned, take them quickly out of the clay, quench evenly in water, and dry them at the fire.

Vật liệu cho bước này:

Mỡ lợn (mỡ lá và mỡ lưng)Mỡ lợn (mỡ lá và mỡ lưng)1 cái
Da dêDa dê1 cái
Chỉ lanhChỉ lanh1 cái
Đất sétĐất sét1 cái

Công cụ cần thiết:

Lò rènLò rèn
Bễ thổiBễ thổi
Kìm rènKìm rèn
Thùng tôi nướcThùng tôi nước
Dao cắt daDao cắt da
7

Troubleshooting

File troubleshooting.

Flow

Loading...
8

History and honest limits

From Theophilus Presbyter, **De Diversis Artibus** (12th century), Book III, chapters XVII-XIX, translated by Robert Hendrie (1847) (checked on the archive.org scan essayuponvarious00hend, pp. 223-225). He gives no sizes, temperatures or tooth spacing. The tools and the case-hardening explanation are ours.

Vật liệu

8

Công cụ yêu cầu

11

Bản thiết kế này làm ra

Blueprint liên quan

Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...