Thread Locker: Tetraethylene Glycol Dimethacrylate with Cumene Hydroperoxide, Set When Air Is Shut Out (Krieble, US 2,895,950)
An anaerobic thread locker. A little cumene hydroperoxide stirred into tetraethylene glycol dimethacrylate stays liquid as long as air reaches it. Shut between threads or plates, away from air, it sets into a tough resin and locks them.
Result: a liquid that keeps a year or more in a half-full bottle and locks steel in 40 minutes to 5 hours, depending on how much catalyst it holds. Heat speeds it up.
Source: V. K. Krieble (American Sealants Company), US 2,895,950 (1959), Example 1. Unknown: how the tetraethylene glycol dimethacrylate is made; the patent uses a bought commercial grade. Not given: bond strength. Picture: Wikimedia Commons.
Cơ bản
2 hours
Hướng dẫn
1
1
Mix in the catalyst
Mix in the catalyst
At room temperature, stir cumene hydroperoxide into commercial-grade tetraethylene glycol dimethacrylate, measuring by volume. Anything from 0.1 to 10 % works; the patent prefers 2 to 10 %. Goggles and gloves: cumene hydroperoxide is an organic peroxide, keep it cool.
Vật liệu cho bước này:
Tetraetylen glycol dimetacrylat100 parts by volume
Cumen hydroperoxit5 parts by volume (0.1-10)Công cụ cần thiết:
Ống đong
Đũa khuấy
Kính bảo hộ kín
Găng tay chống hóa chất2
2
Store it with air
Store it with air
Keep the mixture in a container with air space, preferably polyethylene, which lets air through. Bottles stored half full stayed liquid for a year or more at room temperature.
Công cụ cần thiết:
Chai nhựa3
3
Apply to the threads
Apply to the threads
Put a few drops on the threads before joining the parts. Once air is shut out it sets. Average set times between steel plates at 25-27 °C, by catalyst share: 10 %, 42 min; 5 %, 52 min; 2 1/2 %, 74 min; 1 1/4 %, 84 min. With 0.1 % it takes about five hours.
Công cụ cần thiết:
Bộ pipet và ống nhỏ giọt4
4
Speed it up with heat
Speed it up with heat
Heat sets it faster: the 0.1 % mixture between glass slides, warmed to 100 °C over a steam bath, locked them in five minutes. Ours: a water bath over a burner as the steam bath.
Công cụ cần thiết:
Bể ổn nhiệt
Đèn BunsenVật liệu
2- 100 parts by volumeTạm thời
- 5 parts by volume (0.1-10)Tạm thời
Công cụ yêu cầu
8- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.