White Charcoal Pig Iron: Calcined Magnetic Ore Smelted with Charcoal in a Swedish Blast Furnace (Percy, 1864)
Forge

Tạo bởi

Forge

1. tháng Mười Một 2026NO
2
0
0
0
0

White Charcoal Pig Iron: Calcined Magnetic Ore Smelted with Charcoal in a Swedish Blast Furnace (Percy, 1864)

Sweden's bar iron began in small charcoal blast furnaces fed with roasted magnetic ore. Percy describes the Sten furnace and how the Swedes smelted: slow, with gentle blast, and with no hot blast at all for the best Dannemora iron, whose manganese-rich ore gives a white, crystalline pig made for the finery. Result: white pig iron in iron moulds, 40-60 tons a week; about half the weight of the ore comes out as iron. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 370-375. Picture: Percy's Fig. 54, the Swedish blast furnace.
Chuyên gia
continuous; tapped every 6 hours

Hướng dẫn

1

Calcine the ore

Break the magnetic ore into lumps no bigger than a double fist and roast it carefully in a mine-kiln heated by the waste gas of the furnace. The Swedes always calcine mountain ores, even without sulphur; any sulphur from pyrites is driven off.

Vật liệu cho bước này:

MagnetitMagnetit1 ore

Công cụ cần thiết:

Lò nung quặngLò nung quặng
2

Crush the roasted ore

Crush the calcined ore between grooved cast-iron rolls driven by an overshot water wheel, to pieces of ¼ to 1 cubic inch.

Công cụ cần thiết:

Trục nghiềnTrục nghiền
Guồng nướcGuồng nước
3

Prepare the furnace

Use a charcoal blast furnace of fire-brick in a sand-filled outer shell. Stamp the lower boshes and hearth from 6 parts crushed quartz to 1 part raw fire-clay by measure round a wooden block, and dry it very slowly with a wood fire. It has three water-cooled tuyeres about 2½ inches across.

Công cụ cần thiết:

Lò caoLò cao
4

Set the blast

Blow with a water-driven blowing engine (at Sten three cylinders about 45 inches across, 45-inch stroke) at ½ to 1½ lb per square inch, more for hard charcoal. Keep the blast so slow that the furnace contents take at least 12 hours to pass through. For pig meant for bar iron the blast is warmed only to about 100 °C; the best Dannemora iron is made with cold blast.

Công cụ cần thiết:

Máy thổi gióMáy thổi gió
Guồng nướcGuồng nước
5

Charge charcoal and ore

Charge 30-50 cubic feet of charcoal at a time and 7-10 cwt of ore on top, half spread round the sides and half in the middle, the most siliceous ore first. Dannemora ore needs no flux (other ores take 10-15 % limestone). It takes about 0.8 to 1 ton of charcoal per ton of iron.

Vật liệu cho bước này:

Than củiThan củi1 0.8-1 ton per ton of iron

Công cụ cần thiết:

Lò caoLò cao
6

Tap into iron moulds

Tap every 6 hours and run the metal into iron moulds, not sand. A furnace makes 40-60 tons a week; the cinder runs thin and holds under 1 % iron. Pig from Dannemora ore is white and crystalline, from its manganese.

Công cụ cần thiết:

Khuôn đúc thỏiKhuôn đúc thỏi

Vật liệu

2
  • Tạm thời
  • 1 0.8-1 ton per ton of iron
    Tạm thời

Công cụ yêu cầu

6

Bản thiết kế này làm ra

Blueprint liên quan

Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.