Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
Woody

Tạo bởi

Woody

28. tháng Mười 2026NO
5
0
0
0
0

Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)

A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool. Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Nâng cao
1 day

Hướng dẫn

1

Cut the core and plain strings

Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.

Vật liệu cho bước này:

Dây thép đàn hồi 0,032"Dây thép đàn hồi 0,032"1 as required

Công cụ cần thiết:

Kìm cắtKìm cắt
Kích thước chưa rõKích thước chưa rõ
2

Wind the bronze wrap at room temperature

Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.

Vật liệu cho bước này:

Dây đồng thanh phốt phoDây đồng thanh phốt pho1 as required

Công cụ cần thiết:

Phương pháp quấn chưa rõPhương pháp quấn chưa rõ
Kích thước chưa rõKích thước chưa rõ
Kính bảo hộKính bảo hộ
3

Heat-soak the wound strings

Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.

Công cụ cần thiết:

Lò nướngLò nướng
Nhiệt kế phòng thí nghiệmNhiệt kế phòng thí nghiệm
Bình khí nitơBình khí nitơ
4

Cool and set up the set

Let the strings cool back to room temperature. Make up the set with the plain steel strings.

Công cụ cần thiết:

Kìm cắtKìm cắt

Vật liệu

2

Công cụ yêu cầu

7

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.