Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie

Tạo bởi

Charlie

1. tháng Mười Một 2026DE
2
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)

Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind. Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium. Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
Nâng cao
1 day

Hướng dẫn

1

Mix the oxide with lanthanum

Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.

Vật liệu cho bước này:

Ytterbi oxitYtterbi oxit1 as required

Công cụ cần thiết:

LanthanLanthan
Chén nung tantaliChén nung tantali
2

Reduce in vacuum at 1020 °C

Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.

Công cụ cần thiết:

Lò cảm ứngLò cảm ứng
Bơm chân khôngBơm chân không
Chén nung tantaliChén nung tantali
3

Condense the ytterbium at 200-600 °C

Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.

Công cụ cần thiết:

Tấm ngưng tụ tantalTấm ngưng tụ tantal
4

Melt into ingots under argon

Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.

Công cụ cần thiết:

Chén nung tantaliChén nung tantali
Lò cảm ứngLò cảm ứng
ArgonArgon

Vật liệu

1
  • 1 as required
    Tạm thời

Công cụ yêu cầu

6

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...