Metal Oxide Varistor: Zinc Oxide with 0.2 % Bismuth Oxide, 750 °C, 1.0 mm (Masuyama 1972)
A non-linear resistor: the current through it rises far faster than the voltage across it. Masuyama, Matsuoka and Nishi made one from zinc oxide with a little bismuth oxide: pressed into a disc, sintered, lapped, and given metal electrodes. With 0.2 mole % bismuth oxide, sintered at 750 °C and lapped to 1.0 mm, the disc measured a C-value of 200 at 1 mA and a nonlinearity exponent n of 1.8.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 1. Unknown: how the aluminium is sprayed on and what the silver paint is. The patent calls both well known, so they are linked to unknown heads. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Nâng cao
1 day
Hướng dẫn
1
1
Weigh 99.8 : 0.2 and wet-mill 5 hours
Weigh 99.8 : 0.2 and wet-mill 5 hours
Mix zinc oxide and bismuth oxide 99.8 : 0.2 by moles. Ours, for 10 g: 9.887 g zinc oxide, 0.113 g bismuth oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.
Vật liệu cho bước này:
Bột kẽm oxit9.887 g
Oxit bitmut0.113 gCông cụ cần thiết:
Cân hai đĩa
Máy nghiền bi sắt
Lò sấy2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm².
Công cụ cần thiết:
Máy ép thủy lực
Khuôn ép đĩa
Thước cặp3
3
Sinter 1 hour at 750 °C and furnace-cool
Sinter 1 hour at 750 °C and furnace-cool
Sinter the discs in air for 1 hour at 750 °C, then let them cool in the furnace to room temperature (about 15-30 °C). Masuyama gives 800 to 1200 °C as the best range for zinc oxide with bismuth oxide.
Công cụ cần thiết:
Lò muffle4
4
Lap both faces to 1.0 mm
Lap both faces to 1.0 mm
Lap both faces with 600-mesh silicon carbide until the disc is 1.0 mm thick.
Công cụ cần thiết:
Thước cặp5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.
Vật liệu cho bước này:
Thỏi nhôm1 as required
Sơn bạc dẫn điện1 as required
Dây đồng2 cáiCông cụ cần thiết:
Phương pháp phun kim loại chưa biết
Thước cặpVật liệu
5- 9.887 gTạm thời
- 0.113 gTạm thời
- 1 as requiredTạm thời
- 1 as requiredTạm thời
- 2 cáiTạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.