Metal Oxide Varistor: Zinc Oxide, 0.5 % Bismuth Oxide, 2.5 % Manganese Dioxide, 1350 °C (Masuyama 1972, Ex. 2)
Ed

Tạo bởi

Ed

28. tháng Mười 2026FI
4
0
0
0
0

Metal Oxide Varistor: Zinc Oxide, 0.5 % Bismuth Oxide, 2.5 % Manganese Dioxide, 1350 °C (Masuyama 1972, Ex. 2)

Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with manganese dioxide: 97 % zinc oxide, 0.5 % bismuth oxide and 2.5 % manganese dioxide by moles, sintered at 1350 °C. The disc measured a C-value of 140 at 1 mA and a nonlinearity exponent n of 4.3. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Nâng cao
1 day

Hướng dẫn

1

Weigh 97 : 0.5 : 2.5 and wet-mill 5 hours

Mix zinc oxide, bismuth oxide and manganese dioxide 97 : 0.5 : 2.5 by moles. Ours, for 10 g: 9.46 g zinc oxide, 0.279 g bismuth oxide, 0.26 g manganese dioxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Vật liệu cho bước này:

Bột kẽm oxitBột kẽm oxit9.46 g
Oxit bitmutOxit bitmut0.279 g
Mangan dioxit (pyrolusit)Mangan dioxit (pyrolusit)0.26 g

Công cụ cần thiết:

Cân hai đĩaCân hai đĩa
Máy nghiền bi sắtMáy nghiền bi sắt
Lò sấyLò sấy
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.

Công cụ cần thiết:

Máy ép thủy lựcMáy ép thủy lực
Khuôn ép đĩaKhuôn ép đĩa
Thước cặpThước cặp
3

Sinter 1 hour at 1350 °C and furnace-cool

Sinter the discs in air for 1 hour at 1350 °C, then let them cool in the furnace to room temperature (about 15-30 °C).

Công cụ cần thiết:

Lò muffleLò muffle
4

Lap to 10 mm by 1.5 mm

Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.

Công cụ cần thiết:

Hạt mài cacbua silicHạt mài cacbua silic
Thước cặpThước cặp
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Vật liệu cho bước này:

Thỏi nhômThỏi nhôm1 as required
Sơn bạc dẫn điệnSơn bạc dẫn điện1 as required
Dây đồngDây đồng2 cái

Công cụ cần thiết:

Phương pháp phun kim loại chưa biếtPhương pháp phun kim loại chưa biết
Thước cặpThước cặp

Vật liệu

6

Công cụ yêu cầu

9

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...