3D Printer Filament Extruded from Pellets

Filament is made the way a 3D printer prints, only continuously: dry plastic pellets fall from a hopper onto a turning screw inside a heated barrel, melt as they are carried forward, and are pushed out through a round nozzle. The strand is cooled in air or a water bath, drawn by a puller at a steady speed so it keeps its diameter, and wound on a spool. Commercial 1.75 mm filament is typically held to about ±0.02 mm; a small line should be measured. PETG and many other plastics take up moisture, which makes bubbles and weak prints: makers dry PETG at about 55–70 °C for 5–8 hours, depending on the resin. Melt temperatures follow the resin's datasheet; PETG is usually printed at about 230–260 °C.
Ophakathi
A day per few kilograms

Imiyalelo

1

Dry the pellets

Dry the pellets in a dryer as the resin maker specifies; for PETG about 55–70 °C for 5–8 hours.

Izinto zokwakha zalesi sinyathelo:

Ama-pellet e-PETGAma-pellet e-PETG2 kg
Amagremu wepulasitiki eliphelayo (PLA)Amagremu wepulasitiki eliphelayo (PLA)2 kg
Ama-pellet e-ABSAma-pellet e-ABS2 kg

Amathuluzi adingekayo:

Isomisi sama-pelletIsomisi sama-pellet
Isikali Sedijithali SasekhishiniIsikali Sedijithali Sasekhishini
2

Heat the barrel

Set the barrel's heating zones to rise from the hopper end to the nozzle within the resin's datasheet range and let them settle.

Amathuluzi adingekayo:

Ibharela Ye-extruder Enesikulufu EsisodwaIbharela Ye-extruder Enesikulufu Esisodwa
Isitsha sokufaka amaphilisiIsitsha sokufaka amaphilisi
3

Extrude

Fill the hopper and start the screw slowly. Purge until the strand comes out clear of old material and bubbles.

Amathuluzi adingekayo:

Ibharela Ye-extruder Enesikulufu EsisodwaIbharela Ye-extruder Enesikulufu Esisodwa
Isitsha sokufaka amaphilisiIsitsha sokufaka amaphilisi
Amagilavu Amelana NokushisaAmagilavu Amelana Nokushisa
Izibuko zokuphephaIzibuko zokuphepha
4

Cool and pull

Lead the strand through a water bath or past the fan to the puller. Adjust the puller's speed: faster pulls the strand thinner, slower lets it swell.

Izinto zokwakha zalesi sinyathelo:

AmanziAmanzi50 amalitha

Amathuluzi adingekayo:

Umgqomo omkhulu wepulasitiki wamalitha angu-100Umgqomo omkhulu wepulasitiki wamalitha angu-100
Ifeni yebhokisi (isivinini esiguqukayo)Ifeni yebhokisi (isivinini esiguqukayo)
Isidonsi nesisongi sentamboIsidonsi nesisongi sentambo
5

Measure and wind

Measure the diameter every few metres and wind the filament on a spool. Keep it sealed and dry.

Amathuluzi adingekayo:

I-Caliper Yedijithali Yamayintshi Ayi-6I-Caliper Yedijithali Yamayintshi Ayi-6
Isidonsi nesisongi sentamboIsidonsi nesisongi sentambo
Isikali Sedijithali SasekhishiniIsikali Sedijithali Sasekhishini
6

Troubleshooting

Filament extrusion troubleshooting.

Flow

Loading...

Izinto

4

Amathuluzi Adingekayo

10

CC0 Isizinda Somphakathi

Le blueprint ikhishwe ngaphansi kwe-CC0. Ukhululekile ukukopisha, ukuguqula, ukusabalalisa, nokusebenzisa ngaphandle kwemvume.

Sekela uMenzi ngokuthenga imikhiqizo nge-Blueprint yabo IKhomishane Yomenzi kumiswe ngabathengisi, noma dala inguqulo entsha yale Blueprint bese uyifaka njengoxhumaniso ku-Blueprint yakho ukuze wabelane ngemali engenayo.

Ingxoxo

(0)

Ngena ukuze ujoyine ingxoxo

Kulayishwa amazwana...