Acrylic Polymer Medium: Methyl Methacrylate Emulsified by Persulfate Alone

Acrylic polymer medium is an emulsion of acrylic polymer in water, the binder of acrylic paint. ICI's Renfrew and Gates (US 2,296,403, 1942) found that a persulfate alone both keeps the monomer dispersed and starts it polymerising, so no soap is needed. Their Example 2 stirs 30 parts methyl methacrylate and 20 parts dibutyl phthalate (a plasticiser) hard in 100 parts water with 1 part persulfate at about 80 °C; the batch heats itself to 90-95 °C and gives a very stable emulsion. Using it as paint medium is our choice. The picture: our diagram.
Intermediário
Half a day

Instruções

1

Weigh the charge

Weigh 30 parts methyl methacrylate, 20 parts dibutyl phthalate, 100 parts water and 1 part persulfate (ours: potassium persulfate; the example used lithium persulfate, and the patent names potassium among the alternatives).

Materiais para este passo:

Metacrilato de MetilaMetacrilato de Metila30 parts
Ftalato de dibutilaFtalato de dibutila20 parts
ÁguaÁgua100 parts
Iniciador de persulfatoIniciador de persulfato1 part

Ferramentas necessárias:

Balança de pratosBalança de pratos
Óculos de proteção químicaÓculos de proteção química
Luvas de borrachaLuvas de borracha
2

Stir hard at about 80 °C

Put everything in a flask with a reflux condenser and stir very vigorously at about 80 °C, where it refluxes gently.

Ferramentas necessárias:

Balão de fundo redondoBalão de fundo redondo
Condensador de refluxoCondensador de refluxo
AgitadorAgitador
Banho termostáticoBanho termostático
Placa de aquecimentoPlaca de aquecimento
Termómetro de laboratórioTermómetro de laboratório
Hotte (com conduta)Hotte (com conduta)
3

Let it heat itself

After about half an hour the polymerisation starts giving off heat and the temperature climbs to 90-95 °C on its own. Keep stirring.

Ferramentas necessárias:

AgitadorAgitador
Termómetro de laboratórioTermómetro de laboratório
4

Cool

When the temperature starts to fall, the polymerisation is complete. Stop stirring and let it cool. The result is a very stable emulsion.

Ferramentas necessárias:

Termómetro de laboratórioTermómetro de laboratório

Materiais

4

Ferramentas necessárias

10

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.