Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)

A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh barium carbonate, chalk and iron oxide

Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiais para este passo:

Carbonato de bário (witherita)Carbonato de bário (witherita)15.79 g
Carbonato de cálcio (branco de espanha)Carbonato de cálcio (branco de espanha)2.002 g
Óxido férricoÓxido férrico95.55 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
Respirador P100Respirador P100
2

Mill, presinter and mill as in Example 18

As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
Forno muflaForno mufla
Cadinho com tampa (porcelana)Cadinho com tampa (porcelana)
Tenaz para cadinhoTenaz para cadinho
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
4

Pass through a 1290 °C zone in 5 minutes

Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

3

Ferramentas necessárias

15

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...