Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)

A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh barium carbonate, chalk and iron oxide

Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiais para este passo:

Carbonato de bário (witherita)Carbonato de bário (witherita)59.5 g
Carbonato de cálcio (branco de espanha)Carbonato de cálcio (branco de espanha)30.2 g
Óxido férricoÓxido férrico500 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
Respirador P100Respirador P100
2

Mill with alcohol 15 hours, dry, press

Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
3

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
4

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

3

Ferramentas necessárias

12

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.