Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiais para este passo:

Carbonato de bário (witherita)Carbonato de bário (witherita)99.2 g
Óxido férricoÓxido férrico564.8 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
Respirador P100Respirador P100
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
CrivoCrivo
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Ferramentas necessárias:

Álcool polivinílico em póÁlcool polivinílico em pó
Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
Estufa de secagemEstufa de secagem
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

14

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...