Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1260 °C (Went, Philips 1956, Ex. 28)
A ceramic magnet with both barium and strontium: 0.5 mol barium carbonate and 0.5 mol strontium carbonate to 3 mol iron oxide, milled 15 hours, pressed and passed through a 1260 °C furnace in 20 minutes. Went's rod held 1,665 gauss with a coercive force of 3,235 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 28. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days
Instruções
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 99.2 g barium carbonate (0.5 mol), 73.8 g strontium carbonate (0.5 mol), 483.3 g ferric oxide (3 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Materiais para este passo:
Carbonato de bário (witherita)99.2 g
Carbonato de estrôncio73.8 g
Óxido férrico483.3 gFerramentas necessárias:
Balança de pratos
Luvas de borracha
Respirador P1002
2
Mill with alcohol 15 hours, dry
Mill with alcohol 15 hours, dry
Grind the mixture with alcohol in a ball mill for 15 hours, then dry it.
Ferramentas necessárias:
Moinho de bolas de ferro
Etanol de laboratório, 95 %
Estufa de secagem3
3
Press the powder
Press the powder
Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.
Ferramentas necessárias:
Prensa hidráulica
Matriz de prensagem de discos4
4
Pass through a 1260 °C zone in 20 minutes
Pass through a 1260 °C zone in 20 minutes
Sinter at 1260 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.
Ferramentas necessárias:
Forno tubular
Luvas resistentes ao calor5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Ferramentas necessárias:
Eletroíman
BússolaMateriais
3- Referência
- 73.8 gReferência
- 483.3 gReferência
Ferramentas necessárias
12- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.