Barium-Strontium Ferrite Disc Magnet: 0.21 mol BaCO3, 0.09 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 30)
A ceramic magnet with both barium and strontium: 0.21 mol barium carbonate and 0.09 mol strontium carbonate to 2.7 mol iron oxide, milled as in Example 28, pressed and passed through a 1300 °C furnace in 10 minutes. Went's rod held 1,245 gauss with a coercive force of 2,370 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 30. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days
Instruções
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 41.7 g barium carbonate (0.21 mol), 13.3 g strontium carbonate (0.09 mol), 435.5 g ferric oxide (2.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Materiais para este passo:
Carbonato de bário (witherita)41.7 g
Carbonato de estrôncio13.3 g
Óxido férrico435.5 gFerramentas necessárias:
Balança de pratos
Luvas de borracha
Respirador P1002
2
Mill with alcohol 15 hours, dry
Mill with alcohol 15 hours, dry
As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.
Ferramentas necessárias:
Moinho de bolas de ferro
Etanol de laboratório, 95 %
Estufa de secagem3
3
Press the powder
Press the powder
Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.
Ferramentas necessárias:
Prensa hidráulica
Matriz de prensagem de discos4
4
Pass through a 1300 °C zone in 10 minutes
Pass through a 1300 °C zone in 10 minutes
Sinter in air at 1300 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Ferramentas necessárias:
Forno tubular
Luvas resistentes ao calor5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Ferramentas necessárias:
Eletroíman
BússolaMateriais
3- Referência
- 13.3 gReferência
- 435.5 gReferência
Ferramentas necessárias
12- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.