Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)
Charlie

Criado por

Charlie

28. outubro 2026DE
1
0
0
0
0

Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)

A ceramic magnet with both barium and strontium: 0.09 mol barium carbonate and 0.21 mol strontium carbonate to 2.7 mol iron oxide, milled as in Example 28, pressed and passed through a 1300 °C furnace in 10 minutes. Went's rod held 1,340 gauss with a coercive force of 2,640 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 31. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh the carbonates and iron oxide

Weigh 17.9 g barium carbonate (0.09 mol), 31.0 g strontium carbonate (0.21 mol), 435.5 g ferric oxide (2.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiais para este passo:

Carbonato de bário (witherita)Carbonato de bário (witherita)17.9 g
Carbonato de estrôncioCarbonato de estrôncio31 g
Óxido férricoÓxido férrico435.5 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
Respirador P100Respirador P100
2

Mill with alcohol 15 hours, dry

As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Press the powder

Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
4

Pass through a 1300 °C zone in 10 minutes

Sinter in air at 1300 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

3

Ferramentas necessárias

12

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.