Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper
Charlie

Criado por

Charlie

18. outubro 2026DE
11
0
0
0
0

Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper

Bromide paper is paper coated with silver bromide in gelatin, the printing and enlarging paper of the darkroom. Thorpe (1913) gives a beginner's emulsion: gelatin swelled in potassium bromide solution, silver nitrate made clear with strong ammonia, the two joined under ruby light, ripened, set, washed, and spread on paper as on a glass plate. From the moment the silver goes in, work only by ruby light. Grain and ounce figures are Thorpe's; the gram conversions and the 10-sheet batch are ours. The picture: our own drawing.
Avançado
4 days

Instruções

1

Swell the gelatin

Dissolve 185 grains (12.0 g) of potassium bromide in 5 oz (142 ml) of water. Cover 300 grains (19.4 g) of hard gelatin with it and stir until it softens and swells.

Materiais para este passo:

Brometo de PotássioBrometo de Potássio12 g
Gelatina em póGelatina em pó19.4 g

Ferramentas necessárias:

ÁguaÁgua
Copo de vidro (gobelé)Copo de vidro (gobelé)
Vareta de vidroVareta de vidro
Balança de pratosBalança de pratos
2

Dissolve the silver

Dissolve 231 grains (15.0 g) of silver nitrate in 5 oz (142 ml) of water with gentle heat in the water bath. Add strong ammonia (0.880) a little at a time, stirring, until the precipitate that first forms dissolves again.

Materiais para este passo:

Nitrato de PrataNitrato de Prata15 g

Ferramentas necessárias:

ÁguaÁgua
Solução Forte de Amoníaco (0,880)Solução Forte de Amoníaco (0,880)
Copo de vidro (gobelé)Copo de vidro (gobelé)
Vareta de vidroVareta de vidro
Panela grande (inferior, para banho-maria)Panela grande (inferior, para banho-maria)
3

Melt the gelatin, never above 35 °C

Stand both vessels in the pan of water, never above 35 °C, stirring, until the gelatin is perfectly liquid. Up to here ordinary light is fine.

Ferramentas necessárias:

Panela grande (inferior, para banho-maria)Panela grande (inferior, para banho-maria)
TermómetroTermómetro
Vareta de vidroVareta de vidro
4

Add the silver under ruby light

From now on, ruby light only. Pour the silver solution into the gelatin in a thin stream, stirring all the time. Rinse the silver beaker with about 1 oz (28 ml) of warm water into the emulsion.

Ferramentas necessárias:

Luz de Segurança RubiLuz de Segurança Rubi
Copo de vidro (gobelé)Copo de vidro (gobelé)
Vareta de vidroVareta de vidro
ÁguaÁgua
5

Ripen

Leave the emulsion in the hot water for half to three-quarters of an hour.

Ferramentas necessárias:

Panela grande (inferior, para banho-maria)Panela grande (inferior, para banho-maria)
Luz de Segurança RubiLuz de Segurança Rubi
6

Set in the dark

Pour it into a flat dish, put it in a light-tight box and let it set for at least 24 hours; two or three days is better.

Ferramentas necessárias:

Tabuleiros de cerâmica pouco fundosTabuleiros de cerâmica pouco fundos
Caixa à Prova de LuzCaixa à Prova de Luz
7

Wash through canvas

Scrape the set jelly onto wet coarse canvas and tie it into a bag. Knead it under water so it squeezes through in threads. Pour off the water, cover with fresh, wait 5 minutes and pour off: six to eight times.

Ferramentas necessárias:

EspátulaEspátula
Lona de algodãoLona de algodão
FioFio
ÁguaÁgua
Luz de Segurança RubiLuz de Segurança Rubi
8

Drain and store

Turn the threads onto a strainer covered with a cloth and let the water drain. Rinse with methylated spirit and keep in a lidded jar until coating.

Ferramentas necessárias:

CoadorCoador
Pano de musselinaPano de musselina
Álcool desnaturadoÁlcool desnaturado
Frascos de vidro com tampaFrascos de vidro com tampa
Luz de Segurança RubiLuz de Segurança Rubi
9

Coat the paper

Melt the emulsion in the warm water bath. Lay a sheet of paper flat on a levelled glass slab. Pour emulsion on the middle to cover nearly half the sheet, and spread it to each end with a glass rod 2 inches wider than the sheet, held just off the surface.

Materiais para este passo:

PapelPapel10 folhas

Ferramentas necessárias:

Panela grande (inferior, para banho-maria)Panela grande (inferior, para banho-maria)
Placa de vidroPlaca de vidro
Nível de bolhaNível de bolha
Vareta de vidroVareta de vidro
Luz de Segurança RubiLuz de Segurança Rubi
10

Dry

When the coat has set, move the sheets to a rack in a drying box with a current of air. They dry in 12 to 48 hours. Keep them in the light-tight box.

Ferramentas necessárias:

SecadorSecador
Caixa à Prova de LuzCaixa à Prova de Luz

Materiais

4

Ferramentas necessárias

20

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...