Carbon Electrode: Oil-Coke Pressed with Tar and Baked at 1200° (Thorpe, 1912)
Amorphous carbon electrodes as made for aluminium reduction: oil-coke is selected, ground and calcined, pressed hard with tar as a binder, and baked at about 1200° in a kiln like a pottery kiln, packed in carbon so the surface does not burn.
A good electrode conducts electricity well but heat poorly, is hard, resists surface oxidation, has low porosity and is even throughout. Thorpe gives 25 to 60 amperes per square inch as the permissible current density, though much less is used in practice.
Not given: the tar proportion, the pressure and the sizes.
Source: T. E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), p. 107. Picture: the book's text.
Avançado
Unknown
Instruções
1
1
Grind and calcine the coke
Grind and calcine the coke
Select the oil-coke carefully for low ash, volatile matter and sulphur. Grind it and calcine it. Ours: the ball mill and the kiln for calcining.
Materiais para este passo:
Coque de petróleo1 carefully selectedFerramentas necessárias:
Moinho de bolas de ferro
Forno de alta temperatura2
2
Press with tar
Press with tar
Mix the ground coke with tar as a binder and press it into blocks under high pressure. Ours: a hydraulic press.
Materiais para este passo:
Alcatrão de hulha1 binder
Dimensões desconhecidas1 peçaFerramentas necessárias:
Prensa hidráulica3
3
Bake in carbon
Bake in carbon
Embed the blocks in carbon, which protects their surface from oxidation, and bake them at about 1200° in a kiln built on the lines of a pottery kiln. Ours: petroleum coke as the packing.
Ferramentas necessárias:
Forno de alta temperatura
Coque de petróleoMateriais
3- 1 carefully selectedReferência
- 1 binderReferência
- 1 peçaReferência
Ferramentas necessárias
4- Referência
- Referência
- Referência
- Referência
Este projeto faz
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.