Carbon Steel Strip: Saw Plate Sheared and Annealed Soft

Thin carbon steel strip, soft enough to punch, file and score: the stock for utility-knife blades, hacksaw blades and hole saws, which are hardened only after they are shaped. Start from crucible steel rolled to gauge, cut it into strips with plate shears, then anneal it the way Harcourt's Elementary Forge Practice (1920) gives for tool steel: cherry red, about 1400 °F, and buried in perfectly dry ashes until cold. Cutting strips instead of saw outlines and the file test are ours. The picture is our drawing.
Iniciante
1 day (cooling overnight)

Instruções

1

Roll the plate

Roll crucible steel to the gauge the blades need, as in this blueprint. Stop before the saw outlines are sheared.
2

Mark the strips

Scribe lines along the plate, one strip width apart. The width is whatever the blades need (ours).

Materiais para este passo:

Chapa de aço para lâminas de serraChapa de aço para lâminas de serra1 peça

Ferramentas necessárias:

Ponta de traçarPonta de traçar
Régua de traçarRégua de traçar
3

Shear into strips

Cut along the lines with plate shears, as Grimshaw's saw plates are cut to outline after rolling.

Ferramentas necessárias:

Tesoura de chapaTesoura de chapa
4

Fill a bucket with dry ash

Fill an iron bucket with ashes. They must be perfectly dry, so they conduct heat poorly and the steel cools slowly. Dry slaked lime also works.

Ferramentas necessárias:

Cinza de madeira de leiCinza de madeira de lei
Balde metálicoBalde metálico
5

Heat to cherry red

Heat the strips evenly in the forge to a cherry red, about 1400 °F (760 °C). No hotter: overheated steel goes coarse in the grain and weak.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Tenazes de ferreiroTenazes de ferreiro
Luvas de soldadorLuvas de soldador
6

Bury and leave until cold

Bury the strips in the ash at once and leave them until they are entirely cold, overnight. The slower they cool, the softer they are.

Ferramentas necessárias:

Tenazes de ferreiroTenazes de ferreiro
Balde metálicoBalde metálico
Luvas de soldadorLuvas de soldador
7

Check it is soft

Brush off the ash and stroke a corner with a file: it should bite easily. If it skates, anneal again (our test).

Ferramentas necessárias:

Lima para metalLima para metal

Materiais

1

Ferramentas necessárias

9

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...