Charcoal Finery Iron: the South Wales Process, Ball Hammered into Stamps (Percy, 1864)
Forge

Criado por

Forge

4. novembro 2026NO
9
0
0
0
0

Charcoal Finery Iron: the South Wales Process, Ball Hammered into Stamps (Percy, 1864)

The best iron for charcoal tin-plates, as Percy watched it made at the Morfa Tin-plate Works, Llanelly, on 9 September 1859: pig iron melted under coke in a running-out fire flows into two charcoal fineries, where it is broken up with charcoal, melted down before a cold blast and worked into a ball, which is hammered into a slab and broken into 'stamps'. Charcoal is used because it holds no sulphide of iron, so no sulphur passes into the iron. Source: J. Percy, Metallurgy: Iron and Steel (1864), pp. 581-586. Picture: Fig. 107, the refinery and two charcoal fineries at Morfa.
Avançado
Unknown

Instruções

1

Melt the pig under coke

Melt Pembrokeshire pig iron and Cumberland haematite pig iron together under coke in the running-out fire (melting finery), enough to fill two charcoal fineries: 5 to 6 cwt at Pont-y-Mister; 200 to 250 lb for each finery at Pontypool. Tap it at the bottom so that metal flows first, and keep the slag apart as far as you can. Not given: the proportion of the two pigs.

Materiais para este passo:

Lingotes de ferro-gusaLingotes de ferro-gusa1 5-6 cwt for two fineries
Coque metalúrgicoCoque metalúrgico1 peça

Ferramentas necessárias:

Fogo de refinoFogo de refino
Máquina de soproMáquina de sopro
2

Fill the charcoal fineries

Run the molten metal into the two charcoal fineries, still hot from the last heat. Take off the slag that comes with it as a crust once it has set. Throw in a basket of charcoal and let the cold blast on full.

Materiais para este passo:

Carvão vegetal em pedaços (madeira dura)Carvão vegetal em pedaços (madeira dura)1 a basket per finery, more as needed

Ferramentas necessárias:

Fogo de afinaçãoFogo de afinação
Máquina de soproMáquina de sopro
3

Break up and melt down

Break the friable, half-set metal with an iron bar, mix it with the charcoal and heap it towards the tuyere side, where it melts down before the blast ('sinking a lump'). Throw water on the charcoal at intervals so that it does not burn to waste. Keep loosening and raising the metal from the bottom and the tuyere side.

Ferramentas necessárias:

AtiçadorAtiçador
Fogo de afinaçãoFogo de afinação
ÁguaÁgua
4

Gather the ball

Put back pieces left from the last hammering with a two-pronged fork. Tap off the cinder several times and add charcoal, using the hooks at the sides as fulcra to press loose pieces down onto the ball. Lessen the blast at the end. At Morfa the metal went in at 2 h 10 m and the ball came out at 3 h 23 m.

Ferramentas necessárias:

AtiçadorAtiçador
Fogo de afinaçãoFogo de afinação
5

Hammer the ball into a slab

Put the ball under the cam hammer with the tuyere mark facing the hammerman. Hammer it into a narrow slab, rounded at the ends, about 1 3/4 to 2 1/4 in. thick. While it is hot, nick it across deeply in seven or eight places with a chisel-ended bar under the hammer.

Ferramentas necessárias:

MartineteMartinete
Tenaz de forjaTenaz de forja
6

Quench and break into stamps

Plunge the nicked slab, still red-hot, into cold water to loosen the oxide. Lay it nicks down across a long ribbed anvil and break it with a narrow-ended sledge into 'stamps' of about 26 lb. Set the end pieces apart, sort the rest by soundness, and return broken bits to the next charge.

Ferramentas necessárias:

ÁguaÁgua
Bigorna planaBigorna plana
MarretaMarreta
Tenaz de forjaTenaz de forja

Materiais

3

Ferramentas necessárias

9

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...