Chemical-Resistant Gloves: Butyl Latex over Natural Rubber on a Cotton Liner (Hart & Collyer, US 4,190,685, 1980)
Tex

Criado por

Tex

3. novembro 2026FO
13
0
0
0
0

Chemical-Resistant Gloves: Butyl Latex over Natural Rubber on a Cotton Liner (Hart & Collyer, US 4,190,685, 1980)

Dipped rubber gloves built in layers on a knitted cotton liner: one coat of natural rubber, then five coats of butyl rubber, which lets very little liquid or vapour through. Each coat is dipped from latex on a porcelain hand form, and the whole glove is cured under steam and air pressure. Made in Canada to protect soldiers against chemical warfare agents; worn gloves showed no penetration in 24 hours of field use. Result: flexible, soft chemical-resistant gloves with a comfortable cotton lining. Source: J. A. Hart and J. C. Collyer, US 4,190,685 (1980), latex method. Unknown: sizes, the pigments. Picture: the patent drawing.
Avançado
Unknown

Instruções

1

Sew the cotton liner

Cut knitted or interlock cotton fabric to a glove shape and sew it into a glove. It stretches both ways, soaks up sweat and makes the glove easy to put on and take off. Not given: sizes, the knit.

Materiais para este passo:

Tecido de malha de algodãoTecido de malha de algodão1 liner

Ferramentas necessárias:

TesouraTesoura
Máquina de costuraMáquina de costura
Dimensões desconhecidasDimensões desconhecidas
2

Dip in coagulant

Pull the liner onto a porcelain hand form and flame it to smooth off the surface. Dip it in a 10 % solution of acetic acid in acetone, then turn the form for about 2½ minutes at 24 °C until it is dry. The coagulant sets the latex before it can soak through the cloth.

Materiais para este passo:

Ácido acético (glacial)Ácido acético (glacial)1 10 % in acetone
AcetonaAcetona1 solvent

Ferramentas necessárias:

Forma de luvaForma de luva
Maçarico a propanoMaçarico a propano
3

Dip the natural rubber coat

Dip the liner into natural rubber latex (the patent uses LOTOL 1185) and leave it 5 seconds. Draw it out, turn it upside down and let it dry. Scrub the rubber film with an abrasive cleaner, a brush and water, and dry it again.

Materiais para este passo:

Látex de borracha naturalLátex de borracha natural1 bath
Limpador abrasivoLimpador abrasivo1 as needed

Ferramentas necessárias:

Forma de luvaForma de luva
Escova de esfregarEscova de esfregar
4

Mix the butyl latex bath

Mix, in parts by dry weight: butyl rubber latex 100, sulphur 3, zinc dibutyldithiocarbamate 4, zinc oxide 5, formaldehyde 0.1 as a preservative, a liquid dithiocarbamate curing accelerator 4 (Merac 255 in the patent), and 6.5 of pigments (olive drab in the patent). Not given: the pigments.

Materiais para este passo:

Látex de borracha butílicaLátex de borracha butílica100 parts dry
EnxofreEnxofre3 parts
Dibutilditiocarbamato de zincoDibutilditiocarbamato de zinco4 parts
Óxido de zinco em póÓxido de zinco em pó5 parts
Solução de formaldeído (formol a 37 %)Solução de formaldeído (formol a 37 %)0.1 parts formaldehyde
Acelerador de ditiocarbamato líquidoAcelerador de ditiocarbamato líquido4 parts
Material desconhecidoMaterial desconhecido6.5 parts pigment

Ferramentas necessárias:

AgitadorAgitador
5

Dip five butyl coats

Dip the glove into the butyl latex and draw it out at 10 cm per minute. At once turn the form at about 8 rpm at 24 °C until the film has gelled, then dry it upside down in an oven at 66 °C for 1 hour. Wash, dip and dry again until there are five butyl coats; do not use the abrasive cleaner on the butyl film.

Ferramentas necessárias:

Forma de luvaForma de luva
Estufa de secagemEstufa de secagem
6

Cure and finish

Dry the glove at 66 °C for 1 hour. Cure it for 3 hours in a pressure vessel with 30 psi steam in the jacket (131 °C) and 26 psi air in the chamber. Strip the gloves from the forms while hot; when cool, trim them and wash them in soapy water.

Materiais para este passo:

SabãoSabão1 as needed

Ferramentas necessárias:

Autoclave de bancadaAutoclave de bancada
TesouraTesoura

Materiais

13

Ferramentas necessárias

9

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.