Crucible Furnace: the Brass Founder's Sunk Coke Air Furnace (Larkin, 1907)
The brass founder's crucible furnace: a firebrick-lined pit sunk below the floor, fired with hard coke on an iron grating over the ash-pit, closed by a dome-shaped iron cover and drawn by a flue with a damper. The crucible sits on a firebrick in the middle of the fire, lidded, with coke banked round it, until the metal is melted.
Result: a coke-fired crucible furnace for melting brass and bronze.
Source: J. Larkin, The Practical Brass and Iron Founder's Guide (1907), pp. 96-99. Unknown: all sizes. Picture drawn by Youblob.
Intermediário
Unknown
Instruções
1
1
Build the pit
Build the pit
Sink the furnace below the floor. Line the inside with firebricks set in fireclay; use pure clay (white, opaque, oily to the touch), since iron oxide, magnesia, lime or black lead in brick or clay shortens the furnace's life. Close the ash-pit at the bottom with a hinged iron grating. Not given: sizes.
Materiais para este passo:
Tijolos refratários1 lining
Argila refratária1 jointing
Metal desconhecido1 hinged gratingFerramentas necessárias:
Dimensões desconhecidas2
2
Fit the cover and flue
Fit the cover and flue
Make a dome-shaped cover for the furnace top of cast or wrought iron. Lead a flue from the furnace with a damper in it. Not given: the flue size or height.
Materiais para este passo:
Metal desconhecido1 dome cover, damper
Tubo de chaminé1 flueFerramentas necessárias:
Dimensões desconhecidas3
3
Fire it and melt
Fire it and melt
Burn hard coke broken to lumps the size of a fist. Heat the crucible bottom upwards in the fire, lift it out with the tongs, turn it upright and bed it on a slab of fireclay or a firebrick, put on its lid and bank the fire round it. Put the metal in, close the cover and open the damper for draught until the metal is melted. Black-lead crucibles last longer; clay ones must first be hardened by slowly raising their temperature.
Ferramentas necessárias:
Coque metalúrgico
Cadinho de grafite e argila
Tenaz para cadinhoMateriais
4- 1 liningReferência
- 1 jointingReferência
- 1 dome cover, damperReferência
- 1 flueReferência
Ferramentas necessárias
4- Referência
- Referência
- Referência
- Referência
Materiais de Blueprints conectados
Este projeto faz
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.