Equilateral Glass Prism: Sawn, Ground and Pitch-Polished
Charlie

Criado por

Charlie

19. outubro 2026DE
11
0
0
0
0

Equilateral Glass Prism: Sawn, Ground and Pitch-Polished

A prism splits white light into its colours, so its faces must be optically flat and its angles true. This is how the US arsenals ground prisms in 1918, as F. E. Wright recorded for the Ordnance Department in 1921: saw a blank from optical glass, rough-grind it on iron disks, set a batch of prisms in plaster, fine-grind, and polish on pitch with rouge. Wright's worked example is a right-angle prism; an equilateral prism has three 60° angles, made the same way. The picture: blocking prisms for rough grinding at Frankford Arsenal (Wright 1921, Fig. 77, public domain).
Avançado
2-3 days

Instruções

1

Saw out the blank

Saw a triangular blank from a block of optical glass with a diamond saw, using kerosene as lubricant. Leave several millimetres extra on each face for grinding.

Materiais para este passo:

Vidro ópticoVidro óptico1 as required

Ferramentas necessárias:

Serra de diamanteSerra de diamante
QueroseneQuerosene
Paquímetro digital de 6 polegadasPaquímetro digital de 6 polegadas
Óculos de segurançaÓculos de segurança
2

Rough-grind the faces

Grind one triangular end flat on a rotating iron disk with 90 or 150 mesh grit. Then rough out the three side faces at right angles to it, checking the 60° angles with an angle gauge.

Ferramentas necessárias:

Disco de esmerilhar de ferroDisco de esmerilhar de ferro
Conjunto de grão abrasivo de carboneto de silícioConjunto de grão abrasivo de carboneto de silício
Calibre de ânguloCalibre de ângulo
3

Grind the ends in a batch

Wax 20 or more prisms by their ground ends onto a heated iron disk and grind the other ends together: 90, 150, then 220 mesh, then smoothing grit. Change grit only when the surface is free of scratches. Regrind to the set thickness.

Ferramentas necessárias:

Disco de esmerilhar de ferroDisco de esmerilhar de ferro
Conjunto de grão abrasivo de carboneto de silícioConjunto de grão abrasivo de carboneto de silício
ParafinaParafina
Cera de abelhaCera de abelha
Placa de aquecimentoPlaca de aquecimento
Paquímetro digital de 6 polegadasPaquímetro digital de 6 polegadas
4

Block the prisms in plaster

Set the prisms face down in melted paraffin on a flat iron disk and coat their backs with beeswax. Clamp a ring round them, fill with plaster of Paris and a little Portland cement (10 : 1), and let it harden about 16 hours. Cut the plaster back 1/8 in from the prisms and give it two coats of shellac.

Ferramentas necessárias:

Placa de aquecimentoPlaca de aquecimento
ParafinaParafina
Cera de abelhaCera de abelha
Gesso de estuqueGesso de estuque
Cimento PortlandCimento Portland
Pastilhas de cera de abelhaPastilhas de cera de abelha
5

Fine-grind

Grind the block on a slightly convex plate with wet flour emery (the part that settles out of water between 10 and 60 minutes). After five minutes check with a magnifier: the faces should have an even velvet finish, slightly hollow by less than 0.001 in.

Ferramentas necessárias:

Disco de esmerilhar de ferroDisco de esmerilhar de ferro
Conjunto de grão abrasivo de carboneto de silícioConjunto de grão abrasivo de carboneto de silício
Lupa de joalheiroLupa de joalheiro
6

Polish on pitch

Pour strained pitch with a little rosin 1/4 in deep on an iron tool and cut crossed grooves 1/8 in wide, 1 in apart. Press it true with a rouge-wetted flat. Polish the block with creamy rouge and water on the machine, usually 4–8 hours, running nearly dry at the end.

Ferramentas necessárias:

Breu de alcatrão de madeiraBreu de alcatrão de madeira
Colofónia de pinheiroColofónia de pinheiro
Vermelho de joalheiroVermelho de joalheiro
Máquina de polimento ópticoMáquina de polimento óptico
7

Test for flatness

Lay an optical flat on each face and look at the Newton colours in sodium light (salt in a Bunsen flame). Straight bands to the edge, or one colour over the whole face, mean it is flat.

Ferramentas necessárias:

Plano óptico (padrão)Plano óptico (padrão)
Bico de BunsenBico de Bunsen
SalSal
Lupa de joalheiroLupa de joalheiro
8

Free, clean, check the angle, repeat

Break the plaster away, clean the prisms with benzene and check each angle with the angle gauge. Correct by hand on a flat tool with smoothing grit. Repeat blocking and polishing for every face, smallest face first.

Ferramentas necessárias:

MarteloMartelo
BenzenoBenzeno
Calibre de ânguloCalibre de ângulo
Disco de esmerilhar de ferroDisco de esmerilhar de ferro
Conjunto de grão abrasivo de carboneto de silícioConjunto de grão abrasivo de carboneto de silício

Materiais

1
  • 1 as required
    Referência

Ferramentas necessárias

23

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...