Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 40 °C (McIntire, Dow 1948, Ex. 3, Test 1)
Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 40 °C (200 psi in the tower), it swelled into a log 8 inches across, weighing 7.7 lb per cubic foot, with coarse but uniform cells.
Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avançado
3 days
Instruções
1
1
Charge the tower with polystyrene
Charge the tower with polystyrene
Charge a high-pressure tower with 300 lb of granular polystyrene.
Materiais para este passo:
Poliestireno300 librasFerramentas necessárias:
Reator de pressão
Balança de pratos
Luvas de borracha2
2
Add the propylene fraction
Add the propylene fraction
Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.
Materiais para este passo:
Propileno100 librasFerramentas necessárias:
Garrafa de gás sob pressão
Reator de pressão
Óculos de proteção química3
3
Stand two days at 40 °C
Stand two days at 40 °C
Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.
Ferramentas necessárias:
Reator de pressão
Termómetro de laboratório4
4
Let it out at 40 °C
Let it out at 40 °C
Open the valved outlet near the bottom (3.25 inch in the patent) at 40 °C. The pressure is about 200 psi. The gel flows out and swells into a log 8 inches across, 7.7 lb per cubic foot, with coarse but uniform cells. Close the outlet again.
Ferramentas necessárias:
Reator de pressão
Termómetro de laboratório
Óculos de proteção química
Luvas de borracha5
5
Saw into boards
Saw into boards
When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).
Ferramentas necessárias:
Serrote de marceneiro
Luvas de borrachaFerramentas necessárias
7- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.