Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avançado
3 days

Instruções

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiais para este passo:

PoliestirenoPoliestireno300 libras

Ferramentas necessárias:

Reator de pressãoReator de pressão
Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Materiais para este passo:

PropilenoPropileno100 libras

Ferramentas necessárias:

Garrafa de gás sob pressãoGarrafa de gás sob pressão
Reator de pressãoReator de pressão
Óculos de proteção químicaÓculos de proteção química
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Ferramentas necessárias:

Reator de pressãoReator de pressão
Termómetro de laboratórioTermómetro de laboratório
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Ferramentas necessárias:

Reator de pressãoReator de pressão
Termómetro de laboratórioTermómetro de laboratório
Óculos de proteção químicaÓculos de proteção química
Luvas de borrachaLuvas de borracha
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Ferramentas necessárias:

Serrote de marceneiroSerrote de marceneiro
Luvas de borrachaLuvas de borracha

Materiais

2
  • 300 libras
    Referência
  • 100 libras
    Referência

Ferramentas necessárias

7

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...