Gamelan Bronze Keys: Ten Parts Copper, Three Parts Tin, Cast and Forged
The keys of a saron are bronze bars. Javanese makers give the best gamelan bronze as ten parts copper to three parts tin, melted in a clay bowl (kowi), poured to a blade shape, forged with many kinds of hammer blows, checked, then tuned to the set's scale (Wikipedia, Gamelan production). Charge size, mould and tuning method are ours.
The picture: new saron keys on their frame (Wikimedia Commons).
Avançado
3 days
Instruções
1
1
Weigh ten to three
Weigh ten to three
For six keys weigh 1 kg of copper and 300 g of tin: ten parts copper to three parts tin.
Materiais para este passo:
Lingote de cobre1000 g
Lingote de estanho300 gFerramentas necessárias:
Balança digital de cozinha2
2
Melt in the clay crucible
Melt in the clay crucible
Melt the copper in a clay crucible in the furnace under a strong blast, then add the tin and stir it in.
Materiais para este passo:
Carvão vegetal1 as requiredFerramentas necessárias:
Cadinho de argila fundo
Forno de tijolo
Fole
Tenaz para cadinho
Luvas de soldador
Avental de couro
Protetor facial3
3
Pour the blades
Pour the blades
Pour into an open iron mould to blade-shaped bars, a little longer and thicker than the finished keys. Let them cool.
Ferramentas necessárias:
Tenaz para cadinho
Lingoteira
Luvas de soldador
Avental de couro
Protetor facial4
4
Forge
Forge
Forge each bar to shape on the anvil with a range of hammer blows, working it even along its length.
Ferramentas necessárias:
Forja de ferreiro
Bigorna
Martelo de pena transversal
Tenazes de ferreiro
Luvas de soldador
Avental de couro
Protetor facial5
5
Check and tune
Check and tune
Check each key for cracks. Strike it on soft supports and read its note on the tuner. Grind the ends to raise the note; thin the underside at the middle to lower it. Work in small steps until each key sits on its note.
Ferramentas necessárias:
Afinador cromático e metrónomo (de pinça)
Rebarbadora
Jogo de limas
Protetor facialMateriais
3- 1000 gReferência
- 300 gReferência
- 1 as requiredReferência
Ferramentas necessárias
16- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- 1 vendor sell this, none ship to you yetReferência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.