Glyptal Resin from Glycerin and Phthalic Anhydride: Callahan, 1914

Michael J. Callahan of General Electric patented this in 1914, US 1,108,329 (filed 1912): glycerin and phthalic anhydride heated together give a brittle, transparent, yellowish resin that dissolves in acetone and serves as a varnish. Heated afterwards at a moderate temperature for a long time it turns hard, infusible and insoluble, free of bubbles, with high dielectric strength, for insulating coils and wires. Resins of glycerol and phthalic acid like this were the original alkyds, sold under the name Glyptal.
Avançado
Workshop process

Instruções

1

Weigh out the charge

A carregar o notebook Jupyter…
2

Fuse the charge

Mix two parts by weight of phthalic anhydride with one part of glycerin and heat slowly in a suitable container. At about 100 °C the two fuse to a clear liquid and a slight distillation begins.

Materiais para este passo:

Anidrido ftálicoAnidrido ftálico2 parts by weight
GlicerolGlicerol1 part by weight

Ferramentas necessárias:

Copo de precipitação de borossilicatoCopo de precipitação de borossilicato
Placa de aquecimentoPlaca de aquecimento
TermómetroTermómetro
Vareta de vidroVareta de vidro
3

Hold at 185 °C until distillation stops

Raise the temperature to about 185 °C and keep it there until distillation ceases. Then go on heating at this temperature, or a little higher, about 210 °C, until the first stage of the reaction is complete.

Ferramentas necessárias:

Placa de aquecimentoPlaca de aquecimento
TermómetroTermómetro
4

Test samples and stop in time

Take small samples from the mass and let them cool. As soon as a sample is hard and brittle, without stickiness, stop heating and let the product cool. It sets to a brittle, transparent, somewhat yellowish mass that melts again on heating and dissolves in acetone. Do not heat further: the second stage then starts with a rapid rise in temperature, violent boiling sets in at about 275 °C, and the result is a hard, brittle mass full of cavities.

Ferramentas necessárias:

Vareta de vidroVareta de vidro
TermómetroTermómetro
5

Dissolve it in acetone for varnish

Dissolve the resin in acetone. The solution is clear and can be used as a varnish: impregnate the fibrous covering of coils or wires with it, or paint it on, then evaporate the acetone.

Ferramentas necessárias:

Copo de precipitação de borossilicatoCopo de precipitação de borossilicato
Vareta de vidroVareta de vidro
Pincéis finosPincéis finos
AcetonaAcetona
6

Harden it slowly

Harden the coated or cast resin by heating it at a moderate temperature, preferably about 85 to 100 °C, for a time that depends on the mass: a layer about 0.2 inch thick takes about 15 to 20 hours. In some cases a higher temperature, say 135 °C, can be used. No bubbles form, and the product is hard, dense, infusible and practically insoluble in the usual solvents.

Ferramentas necessárias:

Estufa de secagemEstufa de secagem
TermómetroTermómetro

Materiais

2
  • 2 parts by weight
    Referência
  • 1 part by weight
    Referência

Ferramentas necessárias

7

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...