Steel Files: Forged, Cut and Hardened
Forge

Criado por

Forge

11. outubro 2026NO
33
0
0
0
0

Steel Files: Forged, Cut and Hardened

A file is a bar of high-carbon steel, about 1.0–1.25 % carbon, covered in rows of tiny chisel cuts. The blank is forged with a tang, annealed soft, ground flat, and the teeth are raised one by one with a chisel and hammer: each blow cuts a groove and lifts its edge into a tooth. A single-cut file has one row of parallel cuts, at 65–85° to the length; a double-cut file has a second row crossing the first, for general work the first at 40–45° and the second at 70–80°. The file is then hardened as hard as it will go by quenching it in cold brine, and is never tempered; only the tang is softened so it will not snap. Factories do the same steps by machine.
Avançado
2 days (annealing overnight)

Instruções

1

Forge the blank

At a yellow heat, draw the high-carbon steel to the file's section and forge a narrow, pointed tang at one end.

Materiais para este passo:

Lingote de aço de alto carbonoLingote de aço de alto carbono0.5 kg

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
BigornaBigorna
Martelo de forjaMartelo de forja
Tenaz de forjaTenaz de forja
2

Anneal

Heat the blank no hotter than a blood-red and let it cool very slowly, shut away from the air; factories leave blanks in closed boxes in the furnace for 24–36 hours. Cooled in open air it would harden again.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
3

Straighten and grind

Straighten the blank, grind off the scale and make the faces flat and even, or the teeth will not be uniform.

Ferramentas necessárias:

Mó de afiarMó de afiar
4

Cut the teeth

Hold the chisel at an angle and strike it, then move it a small, regular distance and strike again; each blow raises one tooth. For a double cut, cut the first row (overcut), then a second row crossing it (upcut). To cut the other face, turn the file over on a pewter plate so the finished teeth are not crushed.

Ferramentas necessárias:

Talhadeira de picar limasTalhadeira de picar limas
Martelo de forjaMartelo de forja
BigornaBigorna
Placa de estanho (peltre)Placa de estanho (peltre)
5

Harden

Heat the file evenly to its hardening heat and plunge it into a bath of cold brine, which cools faster than water and leaves it harder. Do not temper it.

Materiais para este passo:

SalSal1 kg

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
BaldeBalde
Tenaz de forjaTenaz de forja
6

Soften the tang

Reheat the tang alone so it is no longer glass-hard: a fully hard tang snaps when the handle is driven on. Clean and oil the file.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Tenaz de forjaTenaz de forja

Materiais

2

Ferramentas necessárias

8

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.