Hard Porcelain Body: Kaolin, Felspar, Flint and Chalk, the Sèvres Paste
Hard porcelain is white kaolin made just fusible enough with ground felspar. Andrew Ure (1839) gives the Sèvres paste: 63–70 parts washed kaolin, 22–15 felspar, about 10 flint powder and 5 chalk, mixed as slips, stiffened on plaster and left to ripen damp for months before it is trodden and used.
The picture: centring porcelain paste on the wheel in the Grand Atelier of the Sèvres manufactory.
Avançado
Days to mix, months to ripen
Instruções
1
1
Calcine and grind the felspar
Calcine and grind the felspar
Pick felspar free of dark mica and rust. Heat it red hot in the kiln and quench it so it crumbles, then crush and grind it very fine with water and sift.
Materiais para este passo:
Bloco de feldspato2 kg
Água10 litrosFerramentas necessárias:
Forno cerâmico
Balde de têmpera
Almofariz e pilão
Moleta
Peneira de malha fina
Luvas resistentes ao calor
Máscara antipoeiras2
2
Flint powder
Flint powder
Calcine and quench flint the same way and grind it to a fine powder with water.
Materiais para este passo:
Nódulo de sílex1 kgFerramentas necessárias:
Forno cerâmico
Balde de têmpera
Moleta
Peneira de malha fina
Máscara antipoeiras3
3
Weigh and mix the slips
Weigh and mix the slips
Weigh the dry kaolin, felspar, flint and chalk in Ure's proportions, stir each into water and mix them into one smooth slip; pass it through a fine sieve.
Materiais para este passo:
Caulino em pó6.65 kg
Carbonato de cálcio (branco de espanha)0.5 kg
Água15 litrosFerramentas necessárias:
Balança de pratos
Cuba
Peneira de malha fina4
4
Stiffen on plaster, ripen
Stiffen on plaster, ripen
Pour the slip onto plaster bats to draw the water out without heat. When it is a soft paste, store it covered and damp for months to ripen.
Ferramentas necessárias:
Bolacha de gesso para olaria5
5
Tread and ball it
Tread and ball it
Before use, work the paste hard on the wedging table (Sèvres trod it barefoot) until even, and keep it in damp balls.
Ferramentas necessárias:
Mesa de amassar barro6
6
Ure's Sèvres paste, scaled
Ure's Sèvres paste, scaled
A carregar o notebook Jupyter…
7
7
Limits
Limits
The recipe and handling are Ure's; calcining the flint and the batch size are ours. Grinding flint and felspar makes fine silica dust that harms the lungs over time: grind wet and wear a mask.
Materiais
5- Referência
- 25 litrosReferência
- 1 kgReferência
- 6.65 kgReferência
- Referência
Ferramentas necessárias
11- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.