Oriented Barium Ferrite Disc Magnet: 10,000 Oersted Field (Gorter, Philips 1956, Ex. 4)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Oriented Barium Ferrite Disc Magnet: 10,000 Oersted Field (Gorter, Philips 1956, Ex. 4)

A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a strong 10,000 oersted field, heated to 500 °C in a 2000 oersted field and sintered at 1280 °C. In the principal direction it held 2,875 gauss with a coercive force of 1,800 oersted and a (BH)max of 1.65 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 4. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
3 days

Instruções

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiais para este passo:

Carbonato de bário (witherita)Carbonato de bário (witherita)450 g
Óxido férricoÓxido férrico2000 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Luvas de borrachaLuvas de borracha
Respirador P100Respirador P100
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Ferramentas necessárias:

Forno tubularForno tubular
Cadinho com tampa (porcelana)Cadinho com tampa (porcelana)
Luvas resistentes ao calorLuvas resistentes ao calor
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Ferramentas necessárias:

Poliacetato de viniloPoliacetato de vinilo
AcetonaAcetona
Balança de pratosBalança de pratos
6

Orient in a 10000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.

Ferramentas necessárias:

Matriz de prensagem de discosMatriz de prensagem de discos
EletroímanEletroíman
Prensa hidráulicaPrensa hidráulica
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Ferramentas necessárias:

Forno tubularForno tubular
EletroímanEletroíman
Luvas resistentes ao calorLuvas resistentes ao calor
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
9

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

15

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.