A strontium ferrite magnet oriented in a magnetic field: strontium carbonate and iron oxide milled, pre-fired 2 hours at 1000 °C, ground fine in an agate mill, then oriented, heated and sintered as in Example 4. In the principal direction it held 2,640 gauss with a coercive force of 2,825 oersted and a (BH)max of 1.63 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
3 days
Instruções
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate and 179 g ferric oxide.
Materiais para este passo:
Carbonato de estrôncio29.5 g
Óxido férrico179 gFerramentas necessárias:
Balança de pratos
Respirador P1002
2
Mill 15 hours with alcohol, dry
Mill 15 hours with alcohol, dry
Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.
Ferramentas necessárias:
Moinho de bolas de ferro
Etanol de laboratório, 95 %
Estufa de secagem3
3
Pre-fire 2 hours at 1000 °C in air
Pre-fire 2 hours at 1000 °C in air
Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.
Ferramentas necessárias:
Forno mufla
Cadinho com tampa (porcelana)
Tenaz para cadinho
Luvas resistentes ao calor4
4
Grind 4 hours in an agate centrifugal mill
Grind 4 hours in an agate centrifugal mill
Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.
Ferramentas necessárias:
Moinho centrífugo de ágata
Etanol de laboratório, 95 %
Estufa de secagem5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Ferramentas necessárias:
Poliacetato de vinilo
Acetona
Balança de pratos6
6
Orient in a 10000 oersted field
Orient in a 10000 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.
Ferramentas necessárias:
Matriz de prensagem de discos
Eletroíman
Prensa hidráulica7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Ferramentas necessárias:
Forno tubular
Eletroíman
Luvas resistentes ao calor8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Ferramentas necessárias:
Forno tubular
Luvas resistentes ao calor9
9
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Ferramentas necessárias:
Eletroíman
BússolaMateriais
2- 29.5 gReferência
- 179 gReferência
Ferramentas necessárias
17- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.