Oriented Strontium Ferrite Disc Magnet: Less Iron Oxide, 10,000 Oersted Field (Gorter, Philips 1956, Ex. 9)

A strontium ferrite magnet with less iron oxide than Example 8, oriented, heated and sintered as in Example 4. In the principal direction it held 2,700 gauss with a coercive force of 2,900 oersted and a (BH)max of 1.67 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 9. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
3 days

Instruções

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g strontium carbonate and 163 g ferric oxide.

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio29.5 g
Óxido férricoÓxido férrico163 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill 15 hours with alcohol, dry

Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Pre-fire 2 hours at 1000 °C in air

Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.

Ferramentas necessárias:

Forno muflaForno mufla
Cadinho com tampa (porcelana)Cadinho com tampa (porcelana)
Tenaz para cadinhoTenaz para cadinho
Luvas resistentes ao calorLuvas resistentes ao calor
4

Grind 4 hours in an agate centrifugal mill

Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder. Example 9 does not say how its powder was pre-fired; ours: as in Example 8.

Ferramentas necessárias:

Moinho centrífugo de ágataMoinho centrífugo de ágata
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Ferramentas necessárias:

Poliacetato de viniloPoliacetato de vinilo
AcetonaAcetona
Balança de pratosBalança de pratos
6

Orient in a 10000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.

Ferramentas necessárias:

Matriz de prensagem de discosMatriz de prensagem de discos
EletroímanEletroíman
Prensa hidráulicaPrensa hidráulica
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Ferramentas necessárias:

Forno tubularForno tubular
EletroímanEletroíman
Luvas resistentes ao calorLuvas resistentes ao calor
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
9

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

17

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...