PTFE Ring: Pressed Cold, Sintered Out of the Mould (Brubaker & Hanford 1946)
PTFE will not flow like other plastics, so it cannot be injection moulded. Du Pont's answer was to press the powder cold into shape, take it out of the mould, and only then heat it above 327 °C. The soft, weak pressing keeps its shape in the furnace and comes out tough. This is their Example IV: a ring 8 in across.
Source: M. M. Brubaker and W. E. Hanford (du Pont), US 2,400,099 (1946), Example IV. The press, die and furnace are ours. Picture drawn by Youblob.
Intermediário
1 day
Instruções
1
1
Fill the ring mould with powder
Fill the ring mould with powder
At room temperature, fill a ring mould with powdered PTFE. The finer the powder, the better the result (the patent).
Materiais para este passo:
Pó de resina de PTFE1 as required to fill the mouldFerramentas necessárias:
Matriz de prensagem de anéis2
2
Press at 1000 psi
Press at 1000 psi
Press it at 1000 lb/sq in into a ring ½ in thick, 8 in outside and 4 in inside diameter. The pressed ring is soft and weak: handle it gently.
Ferramentas necessárias:
Prensa hidráulica
Matriz de prensagem de anéis
Régua3
3
Sinter at 355 °C for 6 hours
Sinter at 355 °C for 6 hours
Take the ring out of the mould and heat it, free-standing, in a furnace at 355 °C for 6 hours. Air is fine; no mould is needed to hold its shape.
Ferramentas necessárias:
Forno mufla
Termopar com mostrador4
4
Quench in cold water
Quench in cold water
Lift the hot ring out and quench it in cold water. It comes out hard and tough. It shrinks a little but stays symmetrical.
Ferramentas necessárias:
Tenazes
Balde de têmperaMateriais
1- 1 as required to fill the mouldReferência
Ferramentas necessárias
7- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.