Rubber Compound: Raw Rubber Washed, Dried and Mixed with Sulphur on Hot Rolls (Thorpe, 1913)

How a rubber works of 1913 turned raw rubber into a 'mixing' ready for shaping and curing: the rubber is washed between corrugated rolls under running water, dried on racks, broken down on hot smooth rolls until plastic, and then worked together with fillers and finally sulphur into an even dough. Very few goods were made of rubber and sulphur alone: pure mixings cost too much and are too soft for most uses. Unknown: which fillers, and how much of them and of sulphur. Thorpe names the kinds of materials but gives no mixing. Source: T. E. Thorpe, Dictionary of Applied Chemistry vol. IV (1913), pp. 586-587. Picture: Fig. 1, a washing machine.
Intermediário
3-4 days drying

Instruções

1

Steep and wash the rubber

Cut the raw rubber into lumps or slabs and steep them for some hours in warm water. Pass them again and again through corrugated, diamond-cut or fluted rolls running at a speed difference of 6 : 4 down to one tooth, with a stream of water on the rubber, until the rough crepe-like sheet is clean and thin.

Materiais para este passo:

Folha de borracha fumadaFolha de borracha fumada1 raw rubber
ÁguaÁgua1 warm, then running

Ferramentas necessárias:

Misturador de dois rolos para borrachaMisturador de dois rolos para borracha
2

Dry on racks

Hang the sheet on racks in a drying room until it holds only about 0.25-0.5 per cent moisture: about 3-4 days at about 80°F with good ventilation. Cooler, drier air is better, as warm rubber turns soft and tacky.

Ferramentas necessárias:

SecadorSecador
3

Break it down

Pass the dry rubber repeatedly through the steam-heated smooth rolls of the mixing machine, which run at different speeds, tightening the rolls gradually until the rubber is thoroughly plastic.

Ferramentas necessárias:

Misturador de dois rolos para borrachaMisturador de dois rolos para borracha
4

Mix in the fillers and sulphur

Add the other materials gradually: reclaimed rubber, ground waste, 'substitute' and other organic fillers first, then the minerals and the sulphur last. Work it into a thoroughly even dough without overworking ('tiring') the rubber.

Materiais para este passo:

Material desconhecidoMaterial desconhecido1 fillers and minerals; not given
Enxofre em póEnxofre em pó1 amount not given

Ferramentas necessárias:

Misturador de dois rolos para borrachaMisturador de dois rolos para borracha

Materiais

4

Ferramentas necessárias

2

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...