Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)
Forge

Criado por

Forge

4. novembro 2026NO
22
0
0
0
0

Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)

The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water. Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel. Not given: sizes and teeth per inch. Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
Avançado
Unknown

Instruções

1

Forge the blank

Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).

Materiais para este passo:

Aço de cadinhoAço de cadinho1 cast steel bar
Dimensões desconhecidasDimensões desconhecidas1 peça

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Tenaz de forjaTenaz de forja
Estampa inferiorEstampa inferior
MarteloMartelo
MarretaMarreta
2

Cut the teeth

On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.

Ferramentas necessárias:

Bigorna de açoBigorna de aço
Correia de couroCorreia de couro
TalhadeiraTalhadeira
MarteloMartelo
Lima para metalLima para metal
3

Cut the other sides

To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.

Ferramentas necessárias:

Solda de estanho-chumboSolda de estanho-chumbo
Bigorna de açoBigorna de aço
TalhadeiraTalhadeira
MarteloMartelo
4

Coat for hardening

Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.

Ferramentas necessárias:

Retorta de ferroRetorta de ferro
SalSal
ÁguaÁgua
5

Harden

Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Coque metalúrgicoCoque metalúrgico
Tenaz de forjaTenaz de forja
ÁguaÁgua
6

Clean and oil

Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.

Ferramentas necessárias:

Coque metalúrgicoCoque metalúrgico
ÁguaÁgua
Água de calÁgua de cal
AzeiteAzeite
TerebintinaTerebintina

Materiais

2

Ferramentas necessárias

17

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...