Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)
Charlie

Criado por

Charlie

31. outubro 2026DE
16
0
0
0
0

Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)

Paper soaked in phenol resin is dried, then cured only part of the way, so the resin is stiff but not yet hard. Lucas did this before the final hot press so the press would not squeeze the resin out of the fibres. Result: a dry, partly cured phenolic sheet that a later coat of phenolic resin can still bond into. Source: Lucas, US 1,470,990 (Western Electric, 1923). Stopping before his final hot press is ours. Not given: the solvent in his resin, paper grade, mercerising strengths. Picture drawn by Youblob.
Intermediário
1 hour

Instruções

1

Dip the paper in phenol resin

Run the paper through a bath of phenol resin of specific gravity about 0.970: about 2 minutes for plain paper, 1 minute or less if mercerised first. Ours: Liquid Bakelite as the resin; Lucas does not say how it was thinned.

Materiais para este passo:

PapelPapel1 as required
Baquelite líquida (produto de condensação fenol-formaldeído)Baquelite líquida (produto de condensação fenol-formaldeído)1 as required

Ferramentas necessárias:

Linha de impregnação de pré-impregnadoLinha de impregnação de pré-impregnado
DensímetroDensímetro
2

Optional: mercerise the paper first

For faster, fuller soaking, first pass the paper through caustic soda, squeeze, wash in water, neutralise in an acid, wash again and dry. Strengths and the acid: not given.

Ferramentas necessárias:

Soda cáustica (hidróxido de sódio)Soda cáustica (hidróxido de sódio)
Linha de impregnação de pré-impregnadoLinha de impregnação de pré-impregnado
3

Dry at about 90 °C

Dry the soaked paper in an oven at about 90 °C, just long enough to dry it.

Ferramentas necessárias:

Estufa de secagemEstufa de secagem
4

Part-cure at 120-130 °C

Pass the dry paper through a curing oven at 120-130 °C for about 10 minutes (Lucas's description; his claim 4 says 125 °C for about 10 seconds). The resin sets as stiff as the fibres, but does not harden through.

Ferramentas necessárias:

Forno de curaForno de cura
5

Dip again for 10-15 seconds and dry

Dip the part-cured paper in phenol resin again for 10-15 seconds, then dry at about 90 °C until it can be wound on a reel. Stop here: the sheet is semi-cured. Lucas's next step, stacking and hot pressing, cures it fully.

Materiais para este passo:

Baquelite líquida (produto de condensação fenol-formaldeído)Baquelite líquida (produto de condensação fenol-formaldeído)1 as required

Ferramentas necessárias:

Linha de impregnação de pré-impregnadoLinha de impregnação de pré-impregnado
Estufa de secagemEstufa de secagem

Materiais

2

Ferramentas necessárias

5

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...