Neodymium Magnets, Sample 11: 62Fe-23B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 11, 62 % iron, 23 % boron and 15 % neodymium by atoms: 10.9 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Especialista
2 days
Instruções
1
1
Weigh sample 11: 62 Fe, 23 B, 15 Nd
Weigh sample 11: 62 Fe, 23 B, 15 Nd
Sample 11 is 62 % iron, 23 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 426.6 g iron, 218.4 g ferroboron, 368.3 g neodymium. Unknown: how these three are made.
Materiais para este passo:
Ferro eletrolítico426.6 g
Ferroboro218.4 g
Neodímio metálico368.3 gFerramentas necessárias:
Balança de pratos2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Ferramentas necessárias:
Forno de indução
Cadinho de argila refratária
Árgon
Garrafa de gás sob pressão
Molde de cobre refrigerado a água
Luvas resistentes ao calor3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Ferramentas necessárias:
Engenho de Pilões
Conjunto de peneiras (malha graduada)
Moinho de bolas de ferro
Óculos de segurança4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Ferramentas necessárias:
Prensa com campo magnético5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 11 measured 6.8 kG remanence, 11.3 kOe coercivity and 10.9 MGOe.
Ferramentas necessárias:
Forno tubular
Árgon
Garrafa de gás sob pressão
Luvas resistentes ao calor6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Ferramentas necessárias:
Método de magnetização desconhecidoMateriais
3- 426.6 gReferência
- 218.4 gReferência
- 368.3 gReferência
Ferramentas necessárias
14- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.