Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)

A strontium ferrite with 0.06 mol strontium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 23. Went's rod held 2,120 gauss with a coercive force of 1,950 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 24. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh the carbonates and iron oxide

Weigh 8.86 g strontium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol), 95.55 g ferric oxide (0.6 mol). The patent prints 81.86 g of strontium carbonate beside 0.06 mol. 0.06 mol is 8.86 g (ours, at 147.63 g per mol), the weight used here.

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio8.86 g
Carbonato de cálcio (branco de espanha)Carbonato de cálcio (branco de espanha)4.004 g
Óxido férricoÓxido férrico95.55 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill with alcohol 4 hours, dry

As in Example 23: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Press at 1.5 t/cm²

Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

3

Ferramentas necessárias

11

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...