Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)

A ferrite with half the strontium replaced by calcium: 0.3 mol strontium carbonate and 0.3 mol calcium carbonate to 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,645 gauss with a coercive force of 2,460 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 27. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh the carbonates and iron oxide

Weigh 44.3 g strontium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol), 500.0 g ferric oxide (3.1 mol).

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio44.3 g
Carbonato de cálcio (branco de espanha)Carbonato de cálcio (branco de espanha)30.2 g
Óxido férricoÓxido férrico500 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill with alcohol 15 hours, dry

Grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Press at 1.5 t/cm²

Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

3

Ferramentas necessárias

11

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...