Strontium Ferrite Disc Magnet: 0.8 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 11)
A strontium ferrite: 0.8 mol strontium carbonate to 3.2 mol iron oxide, milled, bound and formed as in Example 4, and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,730 gauss with a coercive force of 3,090 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 11. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days
Instruções
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 118.1 g strontium carbonate (0.8 mol) and 510.9 g ferric oxide (3.2 mol).
Materiais para este passo:
Carbonato de estrôncio118.1 g
Óxido férrico510.9 gFerramentas necessárias:
Balança de pratos
Respirador P1002
2
Mill with alcohol 15.5 hours, dry and sieve
Mill with alcohol 15.5 hours, dry and sieve
As in Example 4: grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.
Ferramentas necessárias:
Moinho de bolas de ferro
Etanol de laboratório, 95 %
Estufa de secagem
Crivo3
3
Knead with a binder and form
Knead with a binder and form
Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.
Ferramentas necessárias:
Álcool polivinílico em pó
Prensa hidráulica
Matriz de prensagem de discos
Estufa de secagem4
4
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Ferramentas necessárias:
Forno tubular
Luvas resistentes ao calor5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Ferramentas necessárias:
Eletroíman
BússolaMateriais
2- 118.1 gReferência
- 510.9 gReferência
Ferramentas necessárias
13- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.