Strontium Ferrite Disc Magnet: 0.6 mol SrCO3 to 3 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 13)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Strontium Ferrite Disc Magnet: 0.6 mol SrCO3 to 3 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 13)

A strontium ferrite: 0.6 mol strontium carbonate to 3 mol iron oxide, milled, bound and formed as in Example 4, and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,100 gauss with a coercive force of 2,800 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 13. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh strontium carbonate and iron oxide

Weigh 88.6 g strontium carbonate (0.6 mol) and 479.0 g ferric oxide (3 mol).

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio88.6 g
Óxido férricoÓxido férrico479 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill with alcohol 15.5 hours, dry and sieve

As in Example 4: grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
CrivoCrivo
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Ferramentas necessárias:

Álcool polivinílico em póÁlcool polivinílico em pó
Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
Estufa de secagemEstufa de secagem
4

Pass through a 1280 °C zone in 10 minutes

Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

13

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...