Strontium Ferrite Disc Magnet: Presintered, 4 Minutes at 1150 °C (Went, Philips 1956, Ex. 25)
Charlie

Criado por

Charlie

28. outubro 2026DE
0
0
0
0
0

Strontium Ferrite Disc Magnet: Presintered, 4 Minutes at 1150 °C (Went, Philips 1956, Ex. 25)

A strontium ferrite with more strontium: 0.4 mol strontium carbonate to 0.8 mol iron oxide, milled, presintered at 1000 °C, milled again, pressed and passed through a 1150 °C furnace in 4 minutes. Went's rod held 1,200 gauss with a coercive force of 3,710 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 25. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Dry the strontium carbonate and weigh

Dry the strontium carbonate at 100 °C. Weigh 59.05 g of it (0.4 mol) and 127.5 g ferric oxide (0.8 mol).

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio59.05 g
Óxido férricoÓxido férrico127.5 g

Ferramentas necessárias:

Estufa de secagemEstufa de secagem
Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill 7 hours, dry at 110 °C

Grind with alcohol in a ball mill for 7 hours and dry at 110 °C.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
3

Presinter in air at 1000 °C for 4 hours

Fire in air at 1000 °C for 4 hours.

Ferramentas necessárias:

Forno muflaForno mufla
Cadinho com tampa (porcelana)Cadinho com tampa (porcelana)
Tenaz para cadinhoTenaz para cadinho
Luvas resistentes ao calorLuvas resistentes ao calor
4

Mill again, dry, press at 1.5 t/cm²

Grind again 7 hours with alcohol, dry at 110 °C and press at 1.5 tonnes per cm² (ours: discs).

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
5

Pass through a 1150 °C zone in 4 minutes

Sinter at 1150 °C by passing the pieces through a 4 cm hot zone at 10 mm per minute: 4 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

14

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.