A strontium ferrite with much more iron oxide: 0.1 mol strontium carbonate to 1 mol, made as in Example 25 but passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,200 gauss with a coercive force of 3,610 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 26. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avançado
2 days

Instruções

1

Weigh strontium carbonate and iron oxide

Weigh 14.76 g strontium carbonate (0.1 mol) and 159.7 g ferric oxide (1 mol).

Materiais para este passo:

Carbonato de estrôncioCarbonato de estrôncio14.76 g
Óxido férricoÓxido férrico159.7 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Respirador P100Respirador P100
2

Mill, presinter and mill as in Example 25

As in Example 25: grind with alcohol 7 hours, dry at 110 °C, fire in air at 1000 °C for 4 hours, grind again and dry.

Ferramentas necessárias:

Moinho de bolas de ferroMoinho de bolas de ferro
Etanol de laboratório, 95 %Etanol de laboratório, 95 %
Estufa de secagemEstufa de secagem
Forno muflaForno mufla
Cadinho com tampa (porcelana)Cadinho com tampa (porcelana)
Tenaz para cadinhoTenaz para cadinho
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs).

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Ferramentas necessárias:

Forno tubularForno tubular
Luvas resistentes ao calorLuvas resistentes ao calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Ferramentas necessárias:

EletroímanEletroíman
BússolaBússola

Materiais

2

Ferramentas necessárias

14

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...