Redditch Steel Sewing Needles: Point, Stamp, Eye, Harden, Scour and Drill (Tomlinson, 1854)
Forge

Criado por

Forge

14. novembro 2026NO
11
0
0
0
0

Redditch Steel Sewing Needles: Point, Stamp, Eye, Harden, Scour and Drill (Tomlinson, 1854)

How the Redditch needle mills of the 1850s made steel sewing needles, from Tomlinson's Cyclopaedia of Useful Arts: wire cut in double lengths, pointed on grit stones, stamped and punched for two eyes, split, hardened and tempered blue, then scoured bright for days in rolled canvas bundles with emery and oil.
Avançado
About two weeks per lot (scouring alone 50-60 hours)

Instruções

1

Gauge and rates

A carregar o notebook Jupyter…
2

Read the Cyclopaedia of Useful Arts

"The raw material, as received from Birmingham or Sheffield, consists of soft, clean steel wire."
3

Cut and straighten

Cut soft steel wire into lengths of two needles each, about 3 in (76 mm) for size No. 6. Collect several thousand inside two heavy iron rings, heat them to redness, lay them on an iron plate and roll them back and forth with a smooth file between the rings until the grating sound softens: they are then straight.

Materiais para este passo:

Arame de açoArame de aço1 peça

Ferramentas necessárias:

Alicate de corteAlicate de corte
Forja de ferreiroForja de ferreiro
Placa de ferroPlaca de ferro
Limas (lima de mão)Limas (lima de mão)
Tenazes de ferreiroTenazes de ferreiro
4

Point both ends

Grind both ends on a fast grit stone (10-20 in across, by needle size). Spread the wires in the left hand, hold them with the right and roll them so each forms a true cone. Dip them in water to keep them cool. The dust of grit and steel causes grinder's asthma: he urged a mask and a fan-driven ventilating shaft; wear a dust mask and extract the dust.

Ferramentas necessárias:

Mó de afiarMó de afiar
Balde de têmperaBalde de têmpera
Máscara antipoeirasMáscara antipoeiras
5

Stamp the eyes

Lay each blank on the iron bed of the stamp (half a die, on a stone block), push it to the stop, and drop the 12 lb hammer with the other half of the die by its foot lever. One blow gives the grooves and a dent for each of the two eyes.

Ferramentas necessárias:

Martelo de queda com matrizes de forjaMartelo de queda com matrizes de forja
6

Punch the eyes

In a small hand press with two steel points the size of the eye, punch both eyes through. File off the burr from many at once spitted on two fine wires through the eyes, then bend the row back and forth between the spits so it breaks into two rows of single needles. Grip each row in a hand vice and file the heads to shape.

Ferramentas necessárias:

Prensa de puncionarPrensa de puncionar
Limas (lima de mão)Limas (lima de mão)
Porta-brocas de mãoPorta-brocas de mão
7

Straighten soft

Roll each bent needle on a flat steel plate with a smooth steel file turned up at each end; two or three turns straighten it.

Ferramentas necessárias:

Placa de ferroPlaca de ferro
Limas (lima de mão)Limas (lima de mão)
8

Harden and temper

Spread the needles thickly on narrow iron plates, heat them to red in the furnace and plunge them into cold water or oil. Dry them, then heat them on an iron plate over a fire, stirring them with small iron shovels until a blue oxide forms, and take them off at once. Roll them on a steel slab to find the bent ones and straighten those with a hammer on a small anvil.

Materiais para este passo:

Óleo de máquinaÓleo de máquina1 peça

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Placa de ferroPlaca de ferro
Balde de têmperaBalde de têmpera
BigornaBigorna
MarteloMartelo
9

Scour bright

Lay strings across an open wooden tray, a stout canvas on them, and 40,000-50,000 needles lengthwise in it. Sprinkle emery, oil and soft soap, roll it up and wind strong twine round it into a bundle 2-3 ft long and 3-4 in thick. Work it under the weighted slab of a scouring machine, 20-30 strokes a minute, for 50-60 hours (7 or 8 days for the best needles). Every 8 hours renew the canvas, add fresh polishing putty and oil, and wash the needles in soap and water.

Materiais para este passo:

Lona de algodãoLona de algodão1 peça
Pó de esmerilPó de esmeril1 peça
Óleo de máquinaÓleo de máquina1 peça
SabãoSabão1 peça
Pó de polirPó de polir1 peça
Cordel de algodãoCordel de algodão1 peça

Ferramentas necessárias:

Máquina de esfregar peças miúdasMáquina de esfregar peças miúdas
10

Head, drill and finish

Turn all heads one way: press a finger wrapped in rag into the heap and the points that stick draw out. Reject broken ones. Anneal the eyes by bringing a red-hot plate near them until dark blue, then countersink and smooth each eye on both sides with a small fast three-sided steel drill. Finish the points on a small turning hone-stone and polish on wooden wheels covered in buff leather with polishing paste.

Materiais para este passo:

Massa de polirMassa de polir1 peça

Ferramentas necessárias:

Placa de ferroPlaca de ferro
Engenho de furarEngenho de furar
Pedra de amolarPedra de amolar
Roda de polirRoda de polir
11

Troubleshooting

Needle troubleshooting.

Flow

Loading...
12

History and honest limits

From Charles Tomlinson (ed.), **Cyclopaedia of Useful Arts** (1854), vol. II, "Needles" (checked on the archive.org scan cyclopdiaofuse02tomlrich, pp. 321-325). He describes a whole mill; quantities scale down. Metric figures, the dust mask and the tool heads are ours.

Materiais

8

Ferramentas necessárias

17

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.