Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
Woody

Criado por

Woody

28. outubro 2026NO
2
0
0
0
0

Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)

A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool. Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Avançado
1 day

Instruções

1

Cut the core and plain strings

Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.

Materiais para este passo:

Corda de aço para instrumentos 0,032"Corda de aço para instrumentos 0,032"1 as required

Ferramentas necessárias:

Alicate de corteAlicate de corte
Dimensões desconhecidasDimensões desconhecidas
2

Wind the bronze wrap at room temperature

Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.

Materiais para este passo:

Fio de bronze fosforosoFio de bronze fosforoso1 as required

Ferramentas necessárias:

Método de enrolamento desconhecidoMétodo de enrolamento desconhecido
Dimensões desconhecidasDimensões desconhecidas
Óculos de segurançaÓculos de segurança
3

Heat-soak the wound strings

Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.

Ferramentas necessárias:

FornoForno
Termómetro de laboratórioTermómetro de laboratório
Cilindro de nitrogênioCilindro de nitrogênio
4

Cool and set up the set

Let the strings cool back to room temperature. Make up the set with the plain steel strings.

Ferramentas necessárias:

Alicate de corteAlicate de corte

Materiais

2

Ferramentas necessárias

7

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.