Metal Oxide Varistor: Zinc Oxide with Bismuth and Chromic Oxides, 1350 °C (Masuyama 1972)
Ed

Criado por

Ed

28. outubro 2026FI
0
0
0
0
0

Metal Oxide Varistor: Zinc Oxide with Bismuth and Chromic Oxides, 1350 °C (Masuyama 1972)

Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with chromic oxide: 99.0 % zinc oxide, 0.5 % bismuth oxide and 0.5 % chromic oxide by moles, sintered at 1350 °C. The disc measured a C-value of 178 at 1 mA and a nonlinearity exponent n of 14.2. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Avançado
1 day

Instruções

1

Weigh 99.0 : 0.5 : 0.5 and wet-mill 5 hours

Mix zinc oxide, bismuth oxide and chromic oxide 99.0 : 0.5 : 0.5 by moles. Ours, for 10 g: 9.631 g zinc oxide, 0.278 g bismuth oxide, 0.091 g chromic oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Materiais para este passo:

Óxido de zinco em póÓxido de zinco em pó9.631 g
Óxido de bismutoÓxido de bismuto0.278 g
Óxido CrômicoÓxido Crômico0.091 g

Ferramentas necessárias:

Balança de pratosBalança de pratos
Moinho de bolas de ferroMoinho de bolas de ferro
Estufa de secagemEstufa de secagem
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.

Ferramentas necessárias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensagem de discosMatriz de prensagem de discos
PaquímetroPaquímetro
3

Sinter 1 hour at 1350 °C and furnace-cool

Sinter the discs in air at 1350 °C for 1 hour, then let them cool in the furnace to room temperature (about 15-30 °C).

Ferramentas necessárias:

Forno muflaForno mufla
4

Lap to 10 mm by 1.5 mm

Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.

Ferramentas necessárias:

Grão de carboneto de silícioGrão de carboneto de silício
PaquímetroPaquímetro
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Materiais para este passo:

Lingote de alumínioLingote de alumínio1 as required
Tinta condutora de prataTinta condutora de prata1 as required
Fio de cobreFio de cobre2 peças

Ferramentas necessárias:

Método de metalização por aspersão desconhecidoMétodo de metalização por aspersão desconhecido
PaquímetroPaquímetro

Materiais

6

Ferramentas necessárias

9

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...