Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
Charlie

创建者

Charlie

20. 十月 2026DE
2
0
0
0
0

Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass

A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding. The picture: our diagram.
中级
3 days

说明

1

Level the bottom plate

Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.

所需工具:

窗玻璃窗玻璃
木框木框
熟石膏熟石膏
1.5 米水平尺1.5 米水平尺
2

Pour the first 1/2 inch

Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.

此步骤所需材料:

甲基丙烯酸甲酯浆液甲基丙烯酸甲酯浆液3 l

所需工具:

橡胶手套橡胶手套
实验室温度计实验室温度计
3

Pour the next layer and cover

Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.

所需工具:

窗玻璃窗玻璃
4

Heat at 80 °C

Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.

所需工具:

干燥炉干燥炉
实验室温度计实验室温度计
耐热手套耐热手套
5

Spring off the glass

Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.

所需工具:

手工刀手工刀
橡胶手套橡胶手套

材料

1

所需工具

9

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...