Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
Charlie

创建者

Charlie

28. 十月 2026DE
2
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)

A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
高级
2 days

说明

1

Weigh barium carbonate, chalk and iron oxide

Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

此步骤所需材料:

碳酸钡(毒重石)碳酸钡(毒重石)59.5 克
碳酸钙(白垩粉)碳酸钙(白垩粉)30.2 克
氧化铁氧化铁500 克

所需工具:

等臂天平等臂天平
橡胶手套橡胶手套
P100 防毒面具P100 防毒面具
2

Mill with alcohol 15 hours, dry, press

Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.

所需工具:

铁球磨机铁球磨机
乙醇——实验级,95 %乙醇——实验级,95 %
干燥炉干燥炉
液压机液压机
圆片压模圆片压模
3

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

所需工具:

管式炉管式炉
耐热手套耐热手套
4

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

所需工具:

电磁铁电磁铁
指南针指南针

材料

3

所需工具

12

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...