Faraday's Law: The One Process You Can Calculate Exactly

Electroplating is unusual among manufacturing processes: the amount of metal deposited can be calculated exactly, in advance, from the current and the time. Each metal ion needs a fixed number of electrons to become an atom, so the charge that passes is a direct count of the atoms deposited. Faraday worked this out in the 1830s and it has not needed amending. What the calculation does not give for free is the **current efficiency** — the fraction of the current that actually deposits metal rather than splitting water. For nickel it is about 95%; for chromium it is about 15%, which is why chrome plating is slow, hot and extravagant.
中级
3 hours

说明

1

Setting up so the numbers mean something

**The part is the cathode**, connected to the negative terminal. Metal ions in solution are positive, so they are attracted to it and are reduced to metal there. **The anode is usually the same metal being plated**, and it dissolves at the same rate as the cathode gains, keeping the bath concentration constant. That is why a nickel bath has nickel anodes and a copper bath has copper. **An inert anode** — lead, platinised titanium, graphite — is used where a soluble one would not work, chromium being the main case. Then the bath is depleted as plating proceeds and must be topped up. **Measure the current, do not assume it.** A bench supply's display is a guide; a meter in series is the measurement. Every number in this rung depends on the current actually being what it says. **Measure the area properly**, including both faces and the edges of a flat part. A part plated at "1 amp" with its area guessed at half its real value gets half the thickness intended. **Agitate.** Solution next to the cathode is depleted of ions as it plates, and without movement the deposit goes rough and burnt. A magnetic stirrer, air sparging, or moving the work — every real plating bath moves.

此步骤所需材料:

硫酸铜(实验级)硫酸铜(实验级)1 个
铜板铜板2 个
蒸馏水蒸馏水1 个

所需工具:

可调式台式电源可调式台式电源
数字万用表——自动量程、真有效值数字万用表——自动量程、真有效值
硼硅玻璃烧杯硼硅玻璃烧杯
加热磁力搅拌器加热磁力搅拌器
2

The calculation, and the thicknesses actually used

正在加载 Jupyter 笔记本…

所需工具:

台式电脑台式电脑
3

Measuring what actually happened

The calculation predicts; the balance confirms. Doing both is how the current efficiency of a particular bath is discovered, and after that the calculation can be trusted. **Weigh before and after**, dry, on a scale reading to a milligram for a small part. The gain is the metal deposited. **Compare with the prediction.** The ratio is the current efficiency of that bath at that current density and temperature, and it is worth writing on the tank. **An efficiency above 100% means something is wrong** — the part was not dry, or it gained weight some other way, or the current was higher than recorded. It is the same impossible-number rule as a chemical yield. **Measure the thickness directly** where it matters: a micrometer across a flat part before and after, which works down to a few microns; or a magnetic or eddy current gauge, which is what industry uses; or a cross-section under a microscope, which is destructive and definitive. **Expect the thickness to vary across the part**, and that is not an error in the calculation — Faraday's law gives the TOTAL metal deposited, and the distribution is the next rung's subject.

此步骤所需材料:

镍片镍片1 个
低碳钢板低碳钢板1 个

所需工具:

精密天平精密天平
千分尺千分尺
6 英寸数显卡尺6 英寸数显卡尺
4

Running a bath: temperature, pH and what to log

A plating bath is a chemical system with a working window, and drifting outside it degrades the deposit long before the bath stops working. **Temperature.** Higher temperature allows higher current density and gives a softer, less stressed deposit; too cold and the deposit is brittle and burns at modest current. A Watts nickel bath runs at 45 to 60 C. **pH.** Nickel wants about 4.0 to 4.5. Too low and the efficiency falls as more current goes to hydrogen; too high and basic salts precipitate into the deposit as roughness. **Concentration.** Falls as the bath is used if the anodes cannot keep up, and low metal concentration shows up first as burning at the edges. **Additives.** Brighteners, levellers and wetting agents. They are consumed, they break down into products that accumulate, and they are the usual reason a bath that worked last month does not now. **Log every run:** date, part, area, current, time, temperature, pH, and the measured weight gain. Six lines, and they turn "the plating has gone dull" into a curve with a cause. **A Hull cell** is the standard diagnostic: a small tank shaped so one test panel sees a whole range of current densities at once. One panel shows the bath's working range, where it burns and where it is too thin — and it uses a few hundred millilitres of solution.

此步骤所需材料:

六水硫酸镍六水硫酸镍1 个
电镀套件(镍)电镀套件(镍)1 个

所需工具:

实验室温度计实验室温度计
可调式台式电源可调式台式电源
数字万用表——自动量程、真有效值数字万用表——自动量程、真有效值

材料

7

所需工具

9

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...