Forged Ball-Peen Hammer

A 2-pound ball-peen hammer forged from 1½-inch square tool steel; a 6½-inch bar gives two heads. The eye is punched and drifted, the body fullered and rounded so it tapers both ways from a thick centre, then the face is drawn out and swaged and the ball peen rounded in a bottom swage. Both ends are hardened by dipping them in turn, with water dripping on the face, and tempered from the heat held around the eye: dark brown for the face, brown or purple for the peen. The eye cools last, which keeps it tough.
高级
4–6 hours

说明

1

Mark and flatten

Mark the bar with a chisel and centre punch. Flatten the end before punching, or the hole grows too large.

此步骤所需材料:

工具钢方钢工具钢方钢1 个

所需工具:

中心冲中心冲
热錾热錾
铁匠炉铁匠炉
铁砧铁砧
大锤大锤
铁匠钳铁匠钳
2

Punch and drift the eye

Punch the eye at the centre-punch mark, drive in a drift and hammer the bulged sides straight.

所需工具:

热冲子热冲子
扩孔冲子扩孔冲子
锻打锤锻打锤
3

Shape the body

Rough out the shape with top and bottom fullers, then round the body at the anvil's rounded edge with a top fuller and set hammer, thicker at the centre than at the ends.

所需工具:

压槽铁(fuller)压槽铁(fuller)
压肩锤压肩锤
4

Face and peen

Cut the head from the bar from four sides for a square end. Draw out the face, swage it and trim it with a hot chisel; then cut the peen to length, cut off its corners and round it in a bottom swage. Drive the drift through from both sides to taper the eye.

所需工具:

热錾热錾
下型锤(下胎模)下型锤(下胎模)
扩孔冲子扩孔冲子
5

Grind

Grind both ends, rounding the edges of the face slightly so it does not mark hot work.

所需工具:

台式砂轮机台式砂轮机
6

Harden and temper

Heat the whole head slowly to the hardening heat and hold it by a tong jaw in the eye. Lower about 1½ inches of the face into water, then harden the peen the same way while water drips on the face, keeping the eye hot. Polish the ends; take the face to dark brown and the peen to brown or purple, then dip the ends alternately so the eye cools slowly.

所需工具:

铁匠炉铁匠炉
淬火水桶淬火水桶
铁匠钳铁匠钳
金刚砂布金刚砂布
7

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

此步骤所需材料:

硬木手柄料硬木手柄料1 个
硬木楔硬木楔1 个
亚麻籽油亚麻籽油10 毫升

所需工具:

双柄刮刨双柄刮刨
双人横割锯双人横割锯