Measuring the Coating: The Average Is Not the Minimum
Charlie

创建者

Charlie

24. 九月 2026DE
22
0
0
0
0

Measuring the Coating: The Average Is Not the Minimum

A plated layer is usually a few microns thick — too thin to see, too thin for a rule, and thin enough that a specification is written in microns at the worst point. It is nevertheless easy to measure, in several independent ways, and the ways disagree for an informative reason: **weighing gives the average over the whole part, and the specification is about the thinnest place.** The previous rung explains why those two numbers can differ by a factor of several. So both measurements are needed, and they answer different questions: the weight checks the process, and the thin spot checks the part.
中级
2 hours

说明

1

By weight, which needs only a balance

**Weigh dry, before and after.** The gain is the metal deposited, and with the area and the density that is an average thickness directly. **Clean and dry the part fully both times.** Water in a recess weighs more than the coating does, which is the commonest error in this measurement. **Weigh by difference on the same balance**, in the same session if possible. A systematic error that is the same both times cancels; changing balances between the two weighings does not. **The area must be right.** An area underestimated by 20% gives a thickness overestimated by 20%, and it is the larger source of error than the balance. **It is also how current efficiency is measured**, by comparing the gain with Faraday's prediction, so one careful weighing calibrates the whole bath. **It cannot see distribution at all.** A part with half its area at 20 microns and half at nothing weighs exactly the same as one evenly at 10.

此步骤所需材料:

低碳钢板低碳钢板2 个
蒸馏水蒸馏水1 个

所需工具:

精密天平精密天平
6 英寸数显卡尺6 英寸数显卡尺
2

The arithmetic, and what a balance can resolve

正在加载 Jupyter 笔记本…

所需工具:

台式电脑台式电脑
3

The other ways, and what each one can see

**Micrometer, before and after.** Works on a flat part for coatings above a few microns, and it measures the specific spot it is placed on — which is its advantage over weighing. It cannot resolve a 1 micron coating, because the instrument's own repeatability is of that order. **Magnetic gauge.** A magnet is pulled away from the surface and the force measured; a non-magnetic coating on a magnetic substrate holds the magnet further away. Non-destructive, instant, cheap, and the standard method for zinc or nickel on steel. **Eddy current gauge.** The same idea for a non-conductive coating on a non-magnetic metal — anodising on aluminium, mainly. **Cross-section under a microscope.** Cut, mount, polish and etch, then measure the layer directly with a calibrated eyepiece. Destructive, slow, and definitive — it shows the thickness at every point across the section, plus the structure of the deposit and any porosity. **Coulometric stripping.** Dissolve the coating anodically from a known small area and count the charge it takes. Faraday's law run backwards. Accurate to a fraction of a micron, destroys a small spot, and it is the reference method. **Pick the method for the question.** Process control: weigh. A specification at a point: a gauge. A dispute: a cross-section.

此步骤所需材料:

低碳钢板低碳钢板1 个
镍片镍片1 个

所需工具:

千分尺千分尺
精密天平精密天平
放大目镜放大目镜
4

Porosity, which thickness does not measure

A barrier coating protects only if it is continuous. A nickel layer of the right average thickness with pores through it protects the substrate worse than no coating at all, because the tiny exposed area at the bottom of each pore corrodes at an accelerated rate against the large noble cathode around it. **The ferroxyl test** finds pores in a coating on steel. A gel or paper soaked in potassium ferricyanide and sodium chloride is laid on the surface; wherever iron is exposed, a bright Prussian blue spot appears within minutes. The pattern of spots is the pattern of pores. **A salt spray test** is the accelerated corrosion standard: hours to failure in a controlled salt fog. It correlates loosely with service life and it is what specifications quote, because it is repeatable. **Pores come from** a substrate that was not smooth, gas bubbles that clung during plating, particles in the bath, and too thin a deposit — porosity falls sharply with thickness, which is the real reason minimum thicknesses are specified. **This is also why decorative chrome is always over nickel.** The chromium is a third of a micron and unavoidably porous; the nickel underneath is ten microns and is what actually protects. A chrome-plated part that has rusted has usually had its nickel skimped, not its chrome.

此步骤所需材料:

低碳钢板低碳钢板2 个

所需工具:

放大目镜放大目镜
硼硅玻璃烧杯硼硅玻璃烧杯

材料

3

所需工具

6

CC0 公共领域